Brake lining friction material and preparation method thereof

By using friction materials such as sodium hydride and zirconium oxide, combined with hot pressing and heat treatment processes, the problem of rust and adhesion after the car is parked in water has been solved, and the wear resistance and corrosion resistance of the brake lining have been improved.

CN118855899AInactive Publication Date: 2024-10-29HUANGSHAN UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410926831.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

After the car is parked in water, the brake parts are prone to rust and adhesion. The calcium hydroxide added in the existing technology has low solubility in humid environments and cannot effectively prevent rust.

Method used

The brake lining is prepared using friction materials such as sodium hydride, zirconia, aluminum powder and other materials through hot pressing and heat treatment processes to form a protective film and alkaline environment to prevent corrosion.

Benefits of technology

Effectively prevents rust and adhesion of brake parts after the vehicle is parked in water, and improves the wear resistance and corrosion resistance of the brake lining.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a brake lining friction material which comprises the following raw material components in parts by weight: 15-30 parts of phenolic resin, 1-2 parts of sodium hydride, 4 parts of aramid fiber, 2 parts of zinc powder, 7-12 parts of zirconium oxide, 13 parts of potassium titanate, 3 parts of nitrile rubber powder, 7 parts of magnesium oxide, 2 parts of red copper fiber, 6-8 parts of mineral fiber, 9-14 parts of calcium sulfate whisker and 3 parts of graphite. 20-30 parts of precipitated barium sulfate, 2 parts of iron fibers, 4 parts of aluminum powder, 10 parts of carbon fibers and 10 parts of bamboo fibers. The invention further provides a preparation method of the brake lining. The preparation method comprises the steps that the materials are added into a high-speed plow harrow mixer to be evenly mixed, and a mixed material is obtained; loading into a mold for hot pressing to obtain a pressed crude product; and carrying out heat treatment on the pressed crude product according to the following steps. The brake lining prepared from the friction material and the method can effectively prevent brake parts from being rusted and adhered after wading and parking, so that starting locking of a vehicle is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of automobile manufacturing, in particular to a brake lining friction material and a preparation method thereof. Background Art

[0002] At present, with the increasing popularity of automobiles, the cost of automobile manufacturing is gradually decreasing, and the configuration of vehicles is becoming more and more abundant. In terms of the braking system, the electronic parking function that was only configured in higher-end models a few years ago has gradually become popular in low-end cars, and has now almost become a standard configuration for economical passenger cars. The electronic parking brake system replaces the function of the traditional manual parking handle, and has a large parking force, which reduces the risk of slipping due to the insufficient operating force of the traditional mechanical parking handle. However, the electronic parking caliper brake block and friction pad are always in an exposed environment, and the parking force is usually the maximum parking force, so when the friction block is parked in water, the possibility of rust and adhesion between the brake lining and the counterpart (brake disc, brake drum, etc.) is greatly increased. Summary of the invention

[0003] In order to overcome the above defects of the prior art, an embodiment of the present invention provides a brake lining friction material and a preparation method thereof. The technical problem to be solved by the present invention is that the brake parts are prone to rust and adhesion after the car is parked in water.

[0004] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: the friction material includes raw material components and weight proportions as follows: 15-30 parts of phenolic resin, 1-2 parts of sodium hydride, 4 parts of aramid fiber, 2 parts of zinc powder, 7-12 parts of zirconium oxide, 13 parts of potassium titanate, 3 parts of nitrile rubber powder, 7 parts of magnesium oxide, 2 parts of copper fiber, 6-8 parts of mineral fiber, 9-14 parts of calcium sulfate whisker, 3 parts of graphite, 20-30 parts of precipitated barium sulfate, 2 parts of iron fiber, 4 parts of aluminum powder, 10 parts of carbon fiber and 10 parts of bamboo fiber.

[0005] In a preferred embodiment, a method for preparing a brake lining is also provided, wherein the friction material used to prepare the brake lining includes the following raw material components and weight proportions: 15-30 parts of phenolic resin, 1-2 parts of sodium hydride, 4 parts of aramid fiber, 2 parts of zinc powder, 7-12 parts of zirconium oxide, 13 parts of potassium titanate, 3 parts of nitrile rubber powder, 7 parts of magnesium oxide, 2 parts of copper fiber, 6-8 parts of mineral fiber, 9-14 parts of calcium sulfate whisker, 3 parts of graphite, 20-30 parts of precipitated barium sulfate, 2 parts of iron fiber, 4 parts of aluminum powder, 10 parts of carbon fiber, and 10 parts of bamboo fiber; the method is characterized in that the method comprises the following steps:

[0006] S1, adding phenolic resin, sodium hydride, aramid fiber, zinc powder, zirconium oxide, potassium titanate, nitrile rubber powder, magnesium oxide, copper fiber, mineral fiber, calcium sulfate whisker, graphite and precipitated barium sulfate, iron fiber, aluminum powder, 10 parts of carbon fiber and 10 parts of bamboo fiber into a high-speed plow mixer and mixing evenly to obtain a mixture;

[0007] S2, putting the mixed material obtained in step S1 into a mold for hot pressing to obtain a pressed crude product, the hot pressing temperature is 200°C ± 10°C, the hot pressing pressure is 300kg / cm2, and the hot pressing time is 180 seconds ± 5 seconds;

[0008] S3, coarsely grinding the edges and corners of the pressed coarse products;

[0009] S4. Heat treat the pressed crude product according to the following steps:

[0010] (1) placing the pressed crude product in an oven and heating it from room temperature to 200° C., heating it at a uniform rate for 2 hours, and keeping it at 200° C. for 2 hours;

[0011] (2) Cool to below 60°C in the oven and remove from the oven.

[0012] The specific conditions of some raw material components in the present invention are as follows:

[0013] Sodium hydride is an inorganic salt with the chemical formula NaH. It is white to light gray fine crystals formed by the combination of hydrogen and sodium at high temperature. The fineness is above 350 mesh. Sodium hydride is mainly used as a strong base.

[0014] Zinc powder itself is an amphoteric metal. Both zinc and zinc oxide formed by its oxidation will react with the sodium hydroxide aqueous solution to eventually generate sodium metazincate. The sodium metazincate solution is alkaline, thereby achieving the Ph value that maintains the environment.

[0015] Iron fiber is about 4mm in length and 1mm in diameter. Iron fiber can improve wear resistance.

[0016] When heated, aluminum powder reacts with oxygen to generate aluminum oxide, forming a protective film. Aluminum oxide is hard and effectively improves wear resistance.

[0017] Carbon fiber and bamboo fiber can improve the toughness of brake linings.

[0018] Barium sulfate is a white amorphous powder, non-toxic, insoluble in water, and insoluble in acid. It is used as a filler to reinforce the product and can enhance its anti-aging and weather resistance, making the product less prone to aging and becoming brittle.

[0019] Copper fiber is about 4mm in length and 1mm in diameter. Since copper has excellent thermal conductivity, adding it can improve the heat transfer of the brake pad, quickly absorb the heat generated by braking, and prevent the friction surface temperature from rising sharply.

[0020] The rubber powder is nitrile rubber powder with a fineness of about 90 mesh. Adding this component can properly adjust the hardness of the brake pad and improve the braking comfort.

[0021] Zirconia is a fine powder with a fineness of 5μm. Due to its high strength, moderate Mohs hardness, good wear resistance and high melting point, its addition can effectively improve the high-temperature anti-fading performance of the brake pad.

[0022] Calcium sulfate whiskers are fibrous single crystals of calcium sulfate synthesized from raw gypsum through a specific process and formula. They have many excellent physical and chemical properties such as high strength, high modulus, high toughness, high insulation, wear resistance, high temperature resistance, acid and alkali resistance, corrosion resistance, good infrared reflectivity, easy surface treatment, easy to compound with polymers, non-toxicity, etc. The fineness is 700 mesh.

[0023] Technical effects and advantages of the present invention:

[0024] In the prior art, there is also a method of adding calcium hydroxide to the friction material to try to solve the above-mentioned corrosion problem. When the friction material is immersed in water or in a wet state, the calcium hydroxide in the friction material will migrate hydroxide ions to the liquid phase, thereby slowing down the electron loss rate of the mating parts to achieve the effect of slowing down the corrosion process. However, although calcium hydroxide is a strong base with a theoretical Ph value of 12.4, its solubility will decrease with increasing temperature, and its solubility is only 1.65 g / L at 20°C. Moreover, after the friction material is manufactured and formed, the phenolic resin will wrap and solidify each component, so that only the surface calcium hydroxide that provides alkalinity is exposed at the friction interface. Since the solubility of calcium hydroxide is relatively low and the calcium hydroxide aqueous solution is not a strong alkaline solution, when the brake is wading or immersed in a large amount of water, the calcium hydroxide on the surface of the friction plate will dissolve and the Ph value will drop rapidly. At this time, the brake pad itself will accelerate the corrosion. If the vehicle is parked after wading repeatedly, rust and adhesion are very likely to occur.

[0025] The sodium hydride described in the present invention is an inorganic salt with a chemical formula of NaH. It is white to light gray fine crystals and is formed by the combination of hydrogen and sodium at high temperature. Sodium hydride is mainly used as a strong base. Sodium hydride is oxidized to generate sodium oxide and water. Sodium oxide and water continue to react to generate sodium hydroxide. Sodium hydroxide provides sufficient alkaline material for the friction interface, thereby ensuring that the Ph value of the friction interface does not decrease to achieve the effect of delaying rust. Aluminum powder reacts with oxygen when heated to generate aluminum oxide, forming a protective film to effectively prevent water from corroding the brake lining. At the same time, aluminum oxide has a hard texture and effectively improves wear resistance.

[0026] The method of the present invention has the following beneficial effects: it can effectively prevent the brake parts from rusting and sticking after the vehicle is parked in water, and at the same time improve the wear resistance of the brake lining. DETAILED DESCRIPTION

[0027] The present invention will be further described below in conjunction with the embodiments.

[0028] In this embodiment, the friction material used to make the automobile brake lining is prepared in the following proportions: 15-30 parts of phenolic resin, 1-2 parts of sodium hydride, 4 parts of aramid fiber, 2 parts of zinc powder, 7-12 parts of zirconium oxide, 13 parts of potassium titanate, 3 parts of nitrile rubber powder, 7 parts of magnesium oxide, 2 parts of copper fiber, 6-8 parts of mineral fiber, 9-14 parts of calcium sulfate whisker, 3 parts of graphite, 20-30 parts of precipitated barium sulfate, 2 parts of iron fiber, 4 parts of aluminum powder, 10 parts of carbon fiber, and 10 parts of bamboo fiber.

[0029] The specific preparation method comprises the following steps:

[0030] S1, adding phenolic resin, sodium hydride, aramid fiber, zinc powder, zirconium oxide, potassium titanate, nitrile rubber powder, magnesium oxide, copper fiber, mineral fiber, calcium sulfate whisker, graphite and precipitated barium sulfate, iron fiber, aluminum powder, 10 parts of carbon fiber and 10 parts of bamboo fiber into a high-speed plow mixer and mixing evenly to obtain a mixture;

[0031] S2. Put the mixed material obtained in step S1 into a mold and perform hot pressing to obtain a pressed crude product. The hot pressing temperature is 200°C ± 10°C and the hot pressing pressure is 300kg / cm 2 , hot pressing time is 180 seconds ± 5 seconds;

[0032] S3, heat-treating the pressed crude product according to the following steps:

[0033] Roughly grind the edges and corners of the pressed crude products;

[0034] S4. Heat treat the pressed crude product according to the following steps:

[0035] (1) placing the pressed crude product in an oven and heating it from room temperature to 200° C., heating it at a uniform rate for 2 hours, and keeping it at 200° C. for 2 hours;

[0036] (2) Cool to below 60°C in the oven and remove from the oven.

[0037] 1. For brake linings prepared by the friction material and method of the present invention:

[0038] The first step is to soak the friction lining in a large amount of clean water for 1 hour, then immediately install it on the electronic parking brake, load the parking force according to the actual parking state of the vehicle, and keep it at room temperature for 100 hours. After the holding time is over, unload the parking force and measure the torque required to rotate the brake disc at this time. After the test is completed, the disengagement torque is 10N / m, which is much less than the design requirement of no more than 110N / m. There is almost no rust on the contact surface between the friction lining and the brake disc.

[0039] In the second step, the friction lining is immersed in 5% sodium chloride salt water for 1 hour, and then immediately installed on the electronic parking brake, and the parking force is loaded according to the actual parking state of the vehicle, and kept at room temperature for 144 hours. After the holding time is over, the parking force is unloaded and the torque required to rotate the brake disc is measured. After the test is completed, the disengagement torque is 30N / m, which is much less than the design requirement of no more than 110N / m. There is almost no rust on the contact surface between the friction block and the brake disc.

[0040] 2. For the common brake lining in the prior art:

[0041] After comparison and verification according to the first step method above, the disengagement torque of the friction material is 30N / m, there is floating rust on the surface of the brake disc, and a large proportion of rust layer has adhered to the surface of the friction lining.

[0042] After comparison and verification according to the second step method mentioned above, the disengagement torque of the friction material is 160N / m, there is a large amount of floating rust on the surface of the brake disc, and the surface of the friction block is almost completely covered with a rust layer.

[0043] Finally: The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A brake lining friction material, characterized in that: The friction material includes raw material components and weight proportions as follows: 15-30 parts of phenolic resin, 1-2 parts of sodium hydride, 4 parts of aramid fiber, 2 parts of zinc powder, 7-12 parts of zirconium oxide, 13 parts of potassium titanate, 3 parts of nitrile rubber powder, 7 parts of magnesium oxide, 2 parts of copper fiber, 6-8 parts of mineral fiber, 9-14 parts of calcium sulfate whisker, 3 parts of graphite, 20-30 parts of precipitated barium sulfate, 2 parts of iron fiber, 4 parts of aluminum powder, 10 parts of carbon fiber and 10 parts of bamboo fiber.

2. A method for preparing a brake lining, wherein the friction material used to prepare the brake lining comprises the following raw material components and weight proportions: 15-30 parts of phenolic resin, 1-2 parts of sodium hydride, 4 parts of aramid fiber, 2 parts of zinc powder, 7-12 parts of zirconium oxide, 13 parts of potassium titanate, 3 parts of nitrile rubber powder, 7 parts of magnesium oxide, 2 parts of copper fiber, 6-8 parts of mineral fiber, 9-14 parts of calcium sulfate whisker, 3 parts of graphite, 20-30 parts of precipitated barium sulfate, 2 parts of iron fiber, 4 parts of aluminum powder, 10 parts of carbon fiber, and 10 parts of bamboo fiber; characterized in that: The preparation method comprises the following steps: S1. Add phenolic resin, sodium hydride, aramid fiber, zinc powder, zirconium oxide, potassium titanate, nitrile rubber powder, magnesium oxide, copper fiber, mineral fiber, calcium sulfate whisker, graphite and precipitated barium sulfate, iron fiber, aluminum powder, carbon fiber and bamboo fiber into a high-speed plow mixer and mix them evenly to obtain a mixture; S2, putting the mixed material obtained in step S1 into a mold for hot pressing to obtain a pressed crude product, the hot pressing temperature is 200°C ± 10°C, the hot pressing pressure is 300kg / cm2, and the hot pressing time is 180 seconds ± 5 seconds; S3, coarsely grinding the edges and corners of the pressed coarse products; S4. Heat treat the pressed crude product according to the following steps: (1) placing the pressed crude product in an oven and heating it from room temperature to 200° C., heating it at a uniform rate for 2 hours, and keeping it at 200° C. for 2 hours; (2) Cool to below 60°C in the oven and remove from the oven.

Citation Information

Cited By

  • Composite friction material, preparation thereof and application of composite friction material in brake pad

    CN121022027A