Gallium oxide pn heterojunction diode based on p-type Cr2O3 and preparation method thereof
Patent Information
- Application Number
- CN202410863744.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-29
- Publication Date
- 2024-10-29
Smart Images

Figure CN118866979A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of microelectronic technology, and in particular relates to a gallium oxide pn heterojunction diode, which can be used for high-voltage and high-power equipment. Background Art
[0002] With the development of the fourth generation of ultra-wide bandgap semiconductors, gallium oxide materials have gradually become the focus of the new generation of semiconductor materials. Currently, there are five types of gallium oxide materials that can be prepared: α, β, γ, δ and ε. Since the other metastable phases will be converted into β-Ga2O3 during high-temperature processing, the monoclinic β-Ga2O3 has the best thermal stability, and most of the current research work is also centered on β-Ga2O3. β-Ga2O3 has an ultra-large bandgap width of 4.8eV. This feature makes its ionization rate low, so the breakdown field strength is high. The theoretical calculation limit is about 8MV / cm, which is about 20 times higher than the first generation semiconductor Si and one to two times higher than the third generation semiconductor SiC and GaN. In addition, because β-Ga2O3 has a higher electron mobility, dielectric constant and critical electric field strength, its Baliga quality is 3 times that of 4H-SiC and 1.5 times that of GaN. In addition, the theoretical value of the on-resistance of β-Ga2O3 material is very low, so for unipolar devices under the same breakdown voltage conditions, its conduction loss is at least one order of magnitude lower than that of SiC and GaN devices, which is conducive to improving the efficiency of power devices. Therefore, gallium oxide materials have great potential and development prospects in the research and production of power devices.
[0003] There are two main types of gallium oxide diodes: horizontal and vertical. The channel of the device based on the horizontal structure is located on the surface, and the distance between the anode and cathode can be freely defined. Therefore, the distribution of the channel electric field can be well controlled through subsequent processes such as passivation, annealing, and field plate engineering. At present, the research related to gallium oxide horizontal diodes has a breakdown voltage of more than 10kV. However, due to the chip area wasted in regulating the distance between the anode and cathode, and the accompanying sacrifice of the necessary forward performance, the power figure of merit of gallium oxide horizontal devices is often not high. Relatively speaking, the reverse bias electric field of the gallium oxide vertical structure diode is distributed on the bulk material, and the breakdown voltage can be increased by increasing the thickness of the epitaxial layer, which will not waste the chip area, while avoiding the reliability problems caused by the breakdown of the channel surface. In addition, vertical devices are more suitable for large-scale integration and are suitable for the chip market.
[0004] In recent years, gallium oxide vertical structure diodes have been widely studied. A large number of studies based on ion implantation, mesa etching, field plate termination, junction extension termination, Schottky and pn junction composite termination, etc. have been reported by many units, and the power performance of gallium oxide vertical diodes has been improved step by step. Interface research based on cleaning treatment at the mechanism and calculation level, annealing treatment in different atmospheres, etc., is also further supporting the development of gallium oxide diodes. It is well known that the terminal based on pn junction is one of the most effective terminals for power devices. The lack of p-type gallium oxide has led to extensive research on p-type heterojunction materials: nickel oxide, cuprous oxide, iridium oxide, magnesium oxide, p-type silicon, p-type gallium arsenide, etc. Among them, nickel oxide material has a large bandgap width of 3.7eV and a high dielectric constant. The hole concentration can be controlled by changing the oxygen flow ratio during magnetron sputtering, and it has a high compatibility with gallium oxide.
[0005] Patent document with publication number CN116190417A discloses a vertical β-Ga2O3 Schottky barrier diode and a method for manufacturing the same. Figure 1 As shown. Its structure includes from bottom to top: cathode 50, n-type gallium oxide substrate layer 10, n-type gallium oxide epitaxial layer 20, nickel oxide layer 30, nickel oxide layer 60 covered by anode metal, anode metal layer 40, wherein a part of the anode metal layer is on the n-type gallium oxide epitaxial layer, and the other part is on the p-type nickel oxide layer, the anode metal and the n-type gallium oxide epitaxial layer are in Schottky contact; the cathode metal and the n-type gallium oxide substrate layer are in ohmic contact. Although this device can effectively solve the problem that gallium oxide has no p-type doping and only n-type doping. However, since nickel oxide materials are mostly prepared by magnetron sputtering at room temperature, their reliability is low. Studies have shown that the performance of nickel oxide grown at room temperature will have a sharp decline after 35 days, so the reliability of the device is low. Summary of the invention
[0006] The purpose of the present invention is to address the deficiencies of the above-mentioned prior art and to propose a p-type Cr2O3-based gallium oxide pn heterojunction diode and a preparation method thereof, so as to improve device reliability and reduce device leakage current.
[0007] In order to achieve the above object, the technical solution of the present invention is as follows:
[0008] 1. A method for preparing a p-type Cr2O3-based gallium oxide pn heterojunction diode, comprising, from bottom to top: a cathode metal layer (1), a substrate layer (2), an epitaxial layer (3), a p-type doped layer (4), and an anode metal layer (5), characterized in that: the p-type doped layer (4) adopts a multilayer structure consisting of a first layer (41) to an nth layer (4n) from bottom to top, and each layer is composed of a chromium oxide material with a linearly increasing doping concentration, so as to achieve a higher lattice matching degree with the epitaxial layer (3), improve device reliability, and reduce device leakage current, wherein n is an integer ≥1.
[0009] Furthermore, the thickness of each layer of the multi-layer p-type doped layer (4) varies from 10 to 500 nm, and the total thickness is 10 nm to 1 μm; the doping concentration of the first layer (41) is 10 15 cm -3 ~10 16 cm -3 , the doping concentration of the second layer (42) is 10 16 cm -3 ~10 17 cm -3 , ..., the doping concentration of the nth layer (4n) is 10 19 cm -3 ~10 20 cm -3 , the value of n is determined according to the actual use requirements of the device.
[0010] Furthermore, the cathode metal layer (1) is made of any one of Ti / Ni, Ti / Pt, Ti / Al, and Ti / Au.
[0011] Furthermore, the substrate layer (2) has a doping concentration of 10 17 ~10 20 cm -3 , an n+ gallium oxide doped substrate with a thickness of 200 to 1000 microns.
[0012] Furthermore, the epitaxial layer (3) has a doping concentration of 10 15 ~10 17 cm -3 , an n-gallium oxide doped epitaxial layer with a thickness of 1 to 50 microns.
[0013] Furthermore, the anode metal layer (5) is made of any one of Ni / Au, Ni / Pt, Pt / Au and Pd / Au.
[0014] 2. A p-type chromium oxide-based gallium oxide pn heterojunction diode and a preparation method thereof, characterized in that it comprises the following steps:
[0015] 1) cleaning and heat treating the surface of the substrate layer (2), boiling it in trichloroethylene, acetone and anhydrous ethanol for 10 to 15 minutes, cleaning it with deionized water and boiling it for 10 minutes, heating it in a solution of H2SO4:H3PO3=3:1 for 3 to 10 minutes, and then cleaning it in deionized water to eliminate surface dangling bonds, and then removing the surface oxides with a 5% HF solution, and then blowing it dry with a nitrogen gun;
[0016] 2) The substrate layer (2) after cleaning and heat treatment is placed in a reaction chamber, and a HVPE process is used to deposit a layer with a thickness of 1 to 50 μm and a doping concentration of 10 15 cm -3 ~10 17 cm -3 epitaxial layer (3);
[0017] 3) depositing a cathode metal layer (1) on the back side of the substrate by evaporation or magnetron sputtering, and performing rapid annealing at high temperature;
[0018] 4) making a mask on the epitaxial layer (3), and depositing chromium oxide of the p-type doped layer (4) by pulse laser method or magnetron sputtering process, wherein one or more layers may be deposited, and the concentration of chromium oxide in each layer increases from bottom to top;
[0019] 5) placing the sample after the chromium oxide deposition into a chamber of magnetron sputtering or electron beam evaporation to deposit the anode metal layer (5);
[0020] 6) The sample after the anode metal is evaporated is peeled off and placed in an organic solution for cleaning for 5 minutes to 10 minutes to remove excess photoresist residues, thereby completing the device preparation.
[0021] Compared with the prior art, the present invention has the following advantages:
[0022] Firstly, the present invention adopts a heterogeneous pn junction structure, which has a smaller reverse leakage current and a higher breakdown voltage.
[0023] Secondly, since the p-type doped layer adopts a multilayer structure consisting of the first layer to the nth layer from bottom to top, each layer is composed of chromium oxide materials with linearly increasing hole doping concentrations, the first layer of chromium oxide has the smallest hole concentration and fewer defects, and its lattice mismatch with the gallium oxide material is small, reducing the interface state and trap charge density, so that the prepared gallium oxide diode has smaller leakage; the nth layer of chromium oxide has the largest hole concentration, which helps to reduce the contact resistance between the anode metal and the p-type material, so that the forward current of the prepared diode is larger;
[0024] Thirdly, the p-type doped layer used in the present invention has a larger dielectric constant. Therefore, when the heterojunction diode made of chromium oxide and gallium oxide is reverse biased, its electric field distribution is smoother, thus avoiding premature breakdown of the device and improving reliability. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The figure is a schematic diagram of the structure of an existing vertical β-Ga2O3 Schottky barrier diode.
[0026] Figure 2 It is a schematic diagram of the structure of the gallium oxide pn heterojunction diode based on p-type Cr2O3 of the present invention.
[0027] Figure 3 The present invention is a schematic diagram of the process of preparing a p-type Cr2O3-based gallium oxide pn heterojunction diode. DETAILED DESCRIPTION
[0028] The following is a detailed description of the embodiments of the present invention in conjunction with the accompanying drawings:
[0029] Reference Figure 2 The present invention is based on a p-type Cr2O3-based gallium oxide pn heterojunction diode, comprising: a cathode metal layer 1, a substrate layer 2, an epitaxial layer 3, a p-type doped layer 4, and an anode metal layer 5, wherein:
[0030] The substrate layer 2 has a doping concentration of 10 17 ~10 20 cm -3 , n+ gallium oxide material with a thickness of 200 to 1000 microns.
[0031] The epitaxial layer 3 is located on the substrate layer 2 and has a doping concentration of 10 15 ~10 17 cm -3 , n-gallium oxide material with a thickness of 1 to 50 microns.
[0032] The p-type doped layer 4 is located on the epitaxial layer 3 and has a multilayer structure consisting of the first layer to the nth layer from bottom to top. Each layer is a chromium oxide material with a linearly increasing doping concentration. The thickness of each layer is different and ranges from 10 to 500 nm. The total thickness is 10 nm to 1 μm.
[0033] The doping concentration of the first layer 41 is 10 15 cm -3 ~10 16 cm -3 ,
[0034] The doping concentration of the second layer 42 is 10 16 cm -3 ~1017 cm -3 ,……,
[0035] The doping concentration of the nth layer is 10 19 cm -3 ~10 20 cm -3 , n is an integer ≥ 1, and the specific value is determined according to the actual use requirements of the device.
[0036] The anode metal layer 5 is located on the p-type doped layer and is made of any one of Ni / Au, Ni / Pt, Pt / Au, and Pd / Au, wherein the thickness of the first metal layer is 20 to 100 nm, and the thickness of the second metal layer is 30 to 1000 nm.
[0037] The cathode metal layer 1 is located on the lower surface of the substrate layer 2 and is made of any one of Ti / Ni, Ti / Pt, Ti / Al, and Ti / Au. The thickness of the first metal layer is 20 to 100 nm, and the thickness of the second metal layer is 30 to 1000 nm.
[0038] Reference Figure 3 The present invention provides the following three embodiments for preparing p-type Cr2O3-based gallium oxide pn heterojunction diodes:
[0039] Example 1: Preparation of n+ gallium oxide substrate layer with a doping concentration of 10 18 cm -3 , with a thickness of 600 microns and a doping concentration of 1×10 16 cm -3 , thickness is 1 micron, the number of layers of chromium oxide p-type doping layer is 1, the thickness is 20nm, and the doping concentration is 1×10 16 cm -3 p-type chromium oxide / gallium oxide heterojunction diode.
[0040] Step 1: pre-treat the substrate surface.
[0041] The gallium oxide epitaxial wafer was ultrasonically cleaned in acetone, isopropanol, anhydrous ethanol, and deionized water for 5 min in sequence to remove organic matter on the surface;
[0042] Then soak in a solution of H2SO4:H2O2=3:1 for 2 min, and then wash in deionized water to eliminate surface dangling bonds and oxides;
[0043] The oxide on the surface was removed with a 5% HF solution and then blown dry with a nitrogen gun.
[0044] Step 2, making a cathode metal layer, such as Figure 3 (a) shown.
[0045] The pretreated gallium oxide epitaxial wafer was placed with its reverse side facing upward into an electron beam evaporation chamber, the temperature of the reaction chamber was set to room temperature, and Ti and Au film layers were grown in sequence with thicknesses of 20 / 30 nm respectively.
[0046] Step 3: Ohmization of the cathode metal.
[0047] The gallium oxide epitaxial wafer with cathode metal grown was placed in an organic solution for cleaning, and ultrasonically cleaned for 5 min each with acetone, isopropanol, and deionized water in sequence, and then dried with a nitrogen gun;
[0048] The cleaned gallium oxide epitaxial wafer was placed in a rapid annealing furnace and subjected to rapid thermal annealing in a nitrogen atmosphere with a flow rate of 3 sccm, that is, the annealing was performed at a temperature of 490° C. for 45 seconds.
[0049] Step 4: fabricate a p-type doped layer.
[0050] The front side of the gallium oxide epitaxial wafer is photolithographically processed and developed, and the anode area is determined by patterning, such as Figure 3 (b)
[0051] The photolithographic epitaxial wafer was placed in a magnetron sputtering chamber, and the chamber argon flow rate was set to 20 sccm, oxygen flow rate was set to 1 sccm, chamber pressure was set to 0.3 mTorr, temperature was set to room temperature, and sputtering time was set to 3600 s. Magnetron sputtering was used to prepare a doping concentration of 1×10 16 cm -3 , a p-type monolayer chromium oxide with a thickness of 20 nm, such as Figure 3 (c) as shown.
[0052] Step 5, make the anode, such as Figure 3 (d) as shown.
[0053] The sample after the above process is placed in an electron beam evaporation station, and two layers of metal Ni / Au with a thickness of 20 / 30 nm are deposited on the front side of the p-type chromium oxide at an evaporation rate of 0.1 nm / s as an anode.
[0054] Step 6, anode stripping, such as Figure 3 (e) as shown.
[0055] The sample after the above process is immersed in an acetone solution, and the acetone reacts fully with the photoresist on the front side of the gallium oxide epitaxial wafer to remove excess photoresist;
[0056] The sample with the photoresist removed was ultrasonically cleaned in acetone, isopropanol and deionized water for 10 minutes in turn to complete the anode metal stripping and the device preparation was completed.
[0057] Example 2: Preparation of n+ gallium oxide substrate layer with a doping concentration of 10 17 cm -3 , thickness is 1000 microns, and the doping concentration of n-gallium oxide epitaxial layer is 10 15 cm -3 , thickness is 50 microns, the number of chromium oxide p-type doping layers is 2, the first layer thickness is 20nm, the second layer thickness is 10nm, and the doping concentration of the first layer is 1×10 16 cm -3 , the doping concentration of the first layer is 1×10 18 cm -3 Double-layer p-type chromium oxide / gallium oxide heterojunction diode.
[0058] Step 1: pre-treating the substrate surface.
[0059] First, the gallium oxide epitaxial wafer was boiled in acetone, isopropanol, anhydrous ethanol, and deionized water for 10 minutes in turn to remove surface organic matter; then it was immersed in a solution of H2SO4:H2O2=3:1 for 10 minutes, and then washed in deionized water to eliminate surface dangling bonds and oxides; then 5% HF solution was used to remove surface oxides and blown dry with a nitrogen gun.
[0060] Step 2: Prepare the cathode metal layer, such as Figure 3 (a) shown.
[0061] The pre-treated gallium oxide epitaxial wafer was placed with its reverse side facing upward into an electron beam evaporation chamber, the temperature of the reaction chamber was set to room temperature, and Ti and Pt film layers were grown in sequence with thicknesses of 100 / 600 nm, respectively.
[0062] Step three: Ohmization of the cathode metal.
[0063] The gallium oxide epitaxial wafer on which the cathode metal has been grown is placed in an organic solution for cleaning, and is ultrasonically cleaned with acetone, isopropanol, and deionized water for 5 minutes each, and blown dry with a nitrogen gun; the cleaned gallium oxide epitaxial wafer is then placed in a rapid annealing furnace, and the annealing conditions are set to 480°C and 50s, and rapid thermal annealing is performed in a nitrogen atmosphere with a flow rate of 4sccm.
[0064] Step 4: Make two layers of gradually doped p+ regions.
[0065] The front side of the gallium oxide epitaxial wafer is photolithographically processed and developed, and the anode area is determined by patterning, such as Figure 3 As shown in (b), the wafer is placed in a magnetron sputtering chamber. Under the process conditions of argon flow rate of 20 sccm, oxygen flow rate of 2 sccm, chamber pressure of 0.3 mTorr, room temperature, and sputtering time of 3600 s, a doping concentration of 1×1016 cm -3 , a first p-type chromium oxide layer with a thickness of 20 nm; then, under the process conditions of argon flow rate of 20 sccm, oxygen flow rate of 5 sccm, chamber pressure of 0.4 mTorr, temperature of room temperature, and sputtering time of 600 s, magnetron sputtering was used to prepare a doping concentration of 1×10 18 cm -3 , a second layer of p-type chromium oxide with a thickness of 10 nm, such as Figure 3 (c) as shown.
[0066] Step 5: Make the anode, such as Figure 3 (d) as shown.
[0067] The sample after the above process is placed in an electron beam evaporation station, and two layers of metal Pt / Au with a thickness of 100 / 600 nm are deposited on the front side of the p-type chromium oxide at an evaporation rate of 0.13 nm / s as an anode.
[0068] Step 6: Anode stripping, such as Figure 3 (e) as shown.
[0069] The sample that has completed the above process is immersed in an acetone solution to remove excess photoresist; the sample with the photoresist removed is then ultrasonically cleaned in acetone, isopropanol, and deionized water for 8 minutes in turn to strip off excess anode metal, thereby completing device preparation.
[0070] Example 3: Preparation of n+ gallium oxide substrate layer with a doping concentration of 10 20 cm -3 , thickness is 200 microns, and the doping concentration of n-gallium oxide epitaxial layer is 10 17 cm -3 , the thickness is 10 microns, the chromium oxide p-type doping layer is 4 layers, that is, the first layer thickness is 100nm, the second layer thickness is 50nm, the third layer thickness is 20nm, the fourth layer thickness is 10nm, and the doping concentration of the first layer is 1×10 16 cm -3 , the doping concentration of the second layer is 1×10 17 cm -3 , the doping concentration of the third layer is 1×10 18 cm -3 , the doping concentration of the fourth layer is 1×10 19 cm -3 A four-layer p-type chromium oxide / gallium oxide heterojunction diode.
[0071] Step A: pre-treating the surface of the substrate.
[0072] A1) boiling the gallium oxide epitaxial wafer in acetone, isopropanol, anhydrous ethanol and deionized water for 15 minutes in sequence to remove organic matter on the surface;
[0073] A2) After the heat treatment, the gallium oxide epitaxial wafer was immersed in a solution of H2SO4:H2O2=3:1 for 5 minutes, then rinsed in deionized water to eliminate surface dangling bonds and oxides, and then dried with a nitrogen gun.
[0074] Step B, making a cathode metal layer, such as Figure 3 (a) shown.
[0075] The pre-treated gallium oxide epitaxial wafer is placed with its reverse side facing upward in an electron beam evaporation chamber, and a double-layer film of Ti and Ni with thicknesses of 80 / 1000 nm respectively is grown in sequence at room temperature in the reaction chamber.
[0076] Step C, ohmization of the cathode metal.
[0077] C1) The gallium oxide epitaxial wafer on which the cathode metal has been grown is cleaned with acetone, isopropanol, and deionized water in sequence, each ultrasonically for 10 min, and then blown dry with a nitrogen gun;
[0078] C2) The cleaned gallium oxide epitaxial wafer is then placed in an annealing furnace for rapid thermal annealing in a nitrogen atmosphere with a flow rate of 5 sccm, wherein the annealing temperature is 450° C. and the annealing time is 60 s.
[0079] Step D, making four layers of gradually doped p+ regions.
[0080] D1) The front side of the gallium oxide epitaxial wafer is photolithographically processed and developed, and the anode area is determined by patterning, such as Figure 3 (b)
[0081] D2) Place the photolithographic epitaxial wafer into a magnetron sputtering chamber, and use magnetron sputtering to prepare a doping concentration of 1×10 16 cm -3 The first layer of p-type chromium oxide with a thickness of 100 nm, the process conditions of magnetron sputtering of this layer are: the argon flow rate in the chamber is 20 sccm, the oxygen flow rate is 1 sccm, the chamber pressure is 0.3 mTorr, the temperature is room temperature, and the sputtering time is 7200 s.
[0082] D3) Magnetron sputtering was used to prepare a doping concentration of 1×10 17 cm -3 , a second layer of p-type chromium oxide with a thickness of 50 nm, the process conditions of magnetron sputtering of this layer are: argon flow rate of 20 sccm, oxygen flow rate of 4 sccm, chamber pressure of 0.3 mTorr, temperature of room temperature, and sputtering time of 6000 s;
[0083] D4) Magnetron sputtering was used to prepare a doping concentration of 1×10 18 cm -3 , the third layer of p-type chromium oxide with a thickness of 20nm, the process conditions of magnetron sputtering of this layer are: argon flow rate of 20sccm, oxygen flow rate of 5sccm, chamber pressure of 0.4mTorr, temperature of room temperature, and sputtering time of 3600s;
[0084] D5) Magnetron sputtering was used to prepare a doping concentration of 1×10 19 cm -3 The fourth layer of p-type chromium oxide with a thickness of 10 nm is formed. The process conditions of magnetron sputtering of this layer are: argon flow rate is 20 sccm, oxygen flow rate is 10 sccm, chamber pressure is 0.5 mTorr, temperature is room temperature, and sputtering time is 600 s. Figure 3 (c) as shown.
[0085] Step E, making an anode, such as Figure 3 (d) as shown.
[0086] The sample after the above process is placed in an electron beam evaporation station, and metal Ni / Pt with a thickness of 80 / 1000 nm is deposited on the front side of the p-type chromium oxide at an evaporation rate of 0.2 nm / s as an anode.
[0087] Step F, anode stripping, such as Figure 3 (e) as shown.
[0088] F1) placing the sample after the above process into an acetone solution for soaking, so that the acetone and the photoresist on the front side of the gallium oxide epitaxial wafer fully react to remove excess photoresist;
[0089] F2) The sample with the photoresist removed is placed in acetone, isopropanol, and deionized water for ultrasonic cleaning for 5 minutes in turn to strip off excess anode metal, thereby completing device preparation.
[0090] The above are only three embodiments of the present invention, which do not constitute any limitation to the present invention. Obviously, after understanding the content and principle of the present invention, professionals in this field may make various modifications and changes in form and details without departing from the principle and structure of the present invention. For example, in addition to the chromium oxide material used in this example, the p-type doping layer may also use nickel oxide, cuprous oxide, iridium oxide, magnesium oxide, p-type silicon, and p-type gallium arsenide; the anode metal layer may use Pd / Au in addition to Ni / Au, Ni / Pt, and Pt / Au; the cathode metal layer may use Ti / Al in addition to Ti / Ni, Ti / Pt, and Ti / Au. However, these modifications and changes based on the concept of the present invention are still within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a p-type Cr2O3-based gallium oxide pn heterojunction diode, comprising from bottom to top: A cathode metal layer (1), a substrate layer (2), an epitaxial layer (3), a p-type doped layer (4), and an anode metal layer (5), characterized in that the p-type doped layer (4) adopts a multilayer structure consisting of a first layer (41) to an nth layer (4n) from bottom to top, and each layer is respectively composed of a chromium oxide material with a linearly increasing doping concentration to achieve a higher lattice matching degree with the epitaxial layer (3), improve device reliability, and reduce device leakage current, wherein n is an integer ≥1.
2. The diode according to claim 1, characterized in that: The thickness of each layer of the multi-layer p-type doped layer (4) varies from 10 to 100 nm, and the total thickness is 10 nm to 1 μm; the doping concentration of the first layer (41) is 10 15 cm -3 ~10 16 cm -3 , the doping concentration of the second layer (42) is 10 16 cm -3 ~10 17 cm -3 , ..., the doping concentration of the nth layer (4n) is 10 19 cm -3 ~10 20 cm -3 , the value of n is determined according to the actual use requirements of the device.
3. The diode according to claim 1, characterized in that: The cathode metal layer (1) is made of any one of Ti / Ni, Ti / Pt, Ti / Al and Ti / Au.
4. The diode according to claim 1, characterized in that: The substrate layer (2) has a doping concentration of 10 17 ~10 20 cm -3 , an n+ gallium oxide doped substrate with a thickness of 200 to 1000 microns.
5. The diode according to claim 1, characterized in that: The epitaxial layer (3) has a doping concentration of 10 15 ~10 17 cm -3 , an n-gallium oxide doped epitaxial layer with a thickness of 1 to 50 microns.
6. The diode according to claim 1, characterized in that: The anode metal layer (5) is any one of Ni / Au, Ni / Pt, Pt / Au and Pd / Au.
7. A p-type chromium oxide-based gallium oxide pn heterojunction diode and a preparation method thereof, characterized in that: The steps include: 1) cleaning and heat treating the surface of the substrate layer (2), boiling or ultrasonically cleaning it in acetone, isopropanol, and anhydrous ethanol for 5 to 15 minutes, boiling or ultrasonically cleaning it in deionized water for 5 to 15 minutes, heating it in a solution of H2SO4:H2O2=3:1 for 2 to 10 minutes, and then washing it in deionized water to eliminate surface dangling bonds, and then removing surface oxides with a 5% HF solution, and then blowing it dry with a nitrogen gun; 2) The substrate layer (2) after cleaning and heat treatment is placed in a reaction chamber, and a HVPE process is used to deposit a layer with a thickness of 1 to 50 μm and a doping concentration of 10 15 cm -3 ~10 17 cm -3 epitaxial layer (3); 3) depositing a cathode metal layer (1) on the back side of the substrate by evaporation or magnetron sputtering, and performing rapid annealing at high temperature; 4) making a mask on the epitaxial layer (3), and depositing chromium oxide of the p-type doped layer (4) by pulse laser method or magnetron sputtering process, wherein one or more layers may be deposited, and the concentration of chromium oxide in each layer increases from bottom to top; 5) placing the sample after the chromium oxide deposition into a chamber of magnetron sputtering or electron beam evaporation to deposit the anode metal layer (5); 6) The sample after the anode metal is evaporated is peeled off and placed in an organic solution for cleaning for 5 minutes to 10 minutes to remove excess photoresist residues, thereby completing the device preparation.
8. The method according to claim 7, characterized in that The process conditions of step 3) are as follows: The metal of the cathode (3) is Ti / Ni or Ti / Pt or Ti / Al or Ti / Au, wherein the thickness of the first metal layer is 20 to 100 nm, and the thickness of the second metal layer is 30 to 1000 nm; High temperature annealing temperature is 450℃~490℃; High temperature annealing time is 45s to 60s; The high temperature annealing atmosphere is N2 atmosphere with a flow rate of 3 to 5 sccm.
9. The method according to claim 7, characterized in that: The metal in step 5) is Ni / Au or Ni / Pt or Pt / Au or Pd / Au, wherein the thickness of the first metal layer is 20-100 nm, and the thickness of the second metal layer is 30-1000 nm; The metal deposition rate is 0.1nm / s~0.2nm / s.
10. The method according to claim 7, characterized in that In step 4), the process parameters for growing chromium oxide by magnetron sputtering are as follows: The magnetron sputtering target material is chromium or chromium oxide target with a purity of 99.99%; The magnetron sputtering time is 600s to 7200s; The pressure of the reaction chamber is 0.3mTorr~0.5mTorr; The temperature of the reaction chamber is room temperature; The reaction carrier gas is argon and oxygen, and the ratio of argon to oxygen is 20:1 to 2:1.
Citation Information
Patent Citations
Vertical beta-Ga2O3 Schottky barrier diode and preparation method thereof
CN116190417A