Epitaxial preparation process

By forming an insulating dielectric layer at the interface between the silicon substrate and the transition layer, the problems of breakdown and stress control of the nitride epitaxial sheet at high voltage are solved, the voltage withstandness and uniformity of the epitaxial sheet are improved, and the cost and growth time are reduced. Achieve higher quality nitride semiconductor epitaxial sheet production.

CN118919398APending Publication Date: 2024-11-08NINGBO GRAPHENE INNOVATION CENT CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411000292.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Nitride epitaxial sheets are prone to breakdown at high voltages, and stress and warpage are difficult to control when growing thick films, affecting the uniformity and cost of the device.

Method used

By forming an insulating dielectric layer at the interface between the silicon substrate and the transition layer, the silicon material is converted to SiO2 or SiN by using wet or dry oxidation processes, reducing the thickness requirements of the epitaxial layer, increasing the withstand voltage, and reducing growth time and cost.

Benefits of technology

Effectively improve the pressure withstand voltage of nitride epitaxial sheets, reduce growth technology difficulty, improve parameter uniformity and yield, reduce lattice damage, and reduce costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919398A_ABST
    Figure CN118919398A_ABST
Patent Text Reader

Abstract

The invention provides an epitaxy preparation process which is at least used for preparing a silicon substrate nitride semiconductor epitaxy, the structure of a silicon substrate nitride semiconductor epitaxial wafer at least comprises a silicon substrate and a transition layer formed on the silicon substrate, a silicon material at the interface of the silicon substrate and the transition layer is oxidized or nitrided to form an insulating dielectric layer, and the insulating dielectric layer is formed on the silicon substrate. The thickness of the dielectric layer can be adjusted through an oxidation or nitridation process. A silicon material at an interface between an epitaxy and a substrate is converted into an insulating silicon dioxide or silicon nitride material, and a part of the thickness of the substrate Si is converted into a high-voltage-resistant insulating dielectric layer material, so that the voltage resistance of the nitride epitaxial wafer can be effectively improved, and the requirement on the thickness of an epitaxial layer is reduced, so that the difficulty of a growth technology is reduced; the epitaxial growth time can be reduced, and the uniformity of epitaxial parameters is improved, so that the yield of epitaxial wafers and chips is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of semiconductors, and in particular relates to an epitaxial preparation process. Background Art

[0002] As a new type of wide bandgap semiconductor, nitride power devices have high breakdown electric field, more energy saving, more stable physical and chemical properties, can work at higher ambient temperature, have higher switching speed, can reduce the volume and weight of application systems, and other advantages compared with traditional silicon devices. They can be applied to various household appliances, electric vehicles, solar and wind energy and other new energy generation, electric vehicles, robots, intelligent manufacturing industry, large data processing centers and other fields. However, nitride power devices are currently mainly used in the field of medium and low voltage consumer electronics. One of the reasons is that nitride epitaxial materials use heteroepitaxial methods to grow nitride semiconductor thin film materials on large-sized silicon substrates. Because a conductive channel is formed at the interface between the silicon substrate and the nitride epitaxial layer, the device tends to break down first in the vertical direction under high voltage, and the withstand voltage of gallium nitride power devices is limited by the withstand voltage of the epitaxial material in the vertical direction. Increasing the thickness of the epitaxial material can improve the material's withstand voltage accordingly, but due to the mismatch between the silicon substrate and the nitride epitaxial material in terms of lattice size and thermal expansion coefficient, the thicker the epitaxial layer is grown, the greater the stress inside the epitaxial wafer, making it difficult to control the stress and warping of the epitaxial wafer. At the same time, since the warping of the epitaxial wafer also increases accordingly during the growth of the thick film, the growth conditions at different positions of the epitaxial wafer will have greater differences, reducing the uniformity of various parameters of the epitaxial wafer. The warping control problem and the uniformity problem of the epitaxial wafer will affect the yield and cost of the final product. In addition, the thicker the epitaxial material is grown, the longer the growth time required will be. Since epitaxial production equipment is very expensive, this will also increase the cost of the product.

[0003] The invention patent with the patent number "CN108428619A" discloses a method for preparing a nitride epitaxial layer, which includes the following steps: obtaining a silicon substrate; growing a first transition layer on the silicon substrate; using an implantation process to implant oxygen ions at the contact interface between the silicon substrate and the first transition layer to form an oxide layer between the silicon substrate and the first transition layer; and stacking and growing a second transition layer, a channel layer and a barrier layer on the first transition layer after the implantation process to obtain a nitride epitaxial layer. This effectively improves the breakdown voltage of the epitaxial layer in the vertical direction.

[0004] The invention patent with the patent number "CN106847672A" discloses an epitaxial method for high breakdown voltage gallium nitride power materials, including: providing a substrate; forming a buffer layer on the surface of the substrate; performing ion implantation on the buffer layer to insulate the interface state between the buffer layer and the substrate; and forming a gallium nitride layer on the surface of the buffer layer. The ion implantation process requires single-chip processing, and when forming an insulating material of a certain thickness, it is necessary to adjust the implantation energy for multiple implantations, and a subsequent annealing process to repair lattice damage. Summary of the invention

[0005] In order to solve or improve the existing technical problems, the present invention provides an epitaxial preparation process, which is at least used to prepare silicon substrate nitride semiconductor epitaxy. The structure of the silicon substrate nitride semiconductor epitaxial wafer at least includes: a silicon substrate, and a transition layer formed on the silicon substrate, characterized in that the silicon material at the interface between the silicon substrate and the transition layer is oxidized or nitrided to form an insulating dielectric layer.

[0006] Furthermore, a buffer layer, a channel layer and a barrier layer are sequentially arranged above the transition layer.

[0007] Optionally, an AlN insertion layer is included between the channel layer and the barrier layer.

[0008] Optionally, the barrier layer further includes an unintentionally doped GaN cap layer or an in-situ SiN dielectric layer, or an alloy layer of p-type AlGaInN in any proportion.

[0009] Optionally, the transition layer is selected from one of the following materials: gallium nitride, aluminum nitride, indium nitride, or alloy materials or multi-layer stacked structures of the above materials; or 3C-SiC material, SiN material; or first growing a layer of 3C-SiC or SiN material on the surface of the silicon substrate, and then continuing to grow the above-mentioned gallium nitride, aluminum nitride, indium nitride, or alloy materials or multi-layer stacked structures of the above materials.

[0010] Optionally, the oxidation process is selected from one of the following processes: dry oxidation process, wet oxidation process. The dry oxidation process uses oxygen or oxide-containing gas to react with silicon at high temperature to produce SiO2, and the reaction temperature can be 600-1400°C. The wet oxidation process uses wet oxygen or wet oxide gas to react with silicon at high temperature to produce SiO2, and the reaction temperature can be 600-1400°C. Or, other oxidizing gases such as O3, NO, NO2, SO2 are used to oxidize silicon at high temperature to produce SiO2. Or, the substrate is exposed to a plasma atmosphere containing oxygen elements to oxidize the silicon material at the interface between the nitride and the silicon substrate and convert it into SiO2.

[0011] Optionally, the nitriding process is selected from one of the following processes:

[0012] Treating the substrate with a nitrogen-containing gas (e.g., NH3) in a high temperature environment;

[0013] The substrate is exposed to a plasma atmosphere containing N element, so that the silicon material at the interface between the nitride and the silicon substrate is nitrided and converted into SiN.

[0014] Optionally, the buffer layer is made of one of the following materials: AlN, AlGaN, GaN single layer or multi-layer stacked structure, AlN / GaN, AlN / AlGaN, AlGaN / GaN super lattice structure, or a combination of the above structures.

[0015] Optionally, the channel layer is selected from one of the following materials: GaN material, AlGaN, and InGaN material.

[0016] Optionally, the barrier layer is selected from one of the following materials: AlGaN layer, AlN layer, AlInN, AlInGaN, or a plurality of superpositions of the above material layers.

[0017] Compared with the prior art, the present invention provides an epitaxial preparation process, which has the following beneficial effects: by converting the silicon material at the interface between the epitaxial and the substrate into insulating silicon dioxide or silicon nitride material, and converting a part of the thickness of the substrate Si into a high-voltage insulating dielectric layer material, the voltage resistance of the nitride epitaxial wafer can be effectively improved, and the requirements for the thickness of the epitaxial layer are reduced, thereby reducing the difficulty of the growth technology, and the epitaxial growth time can be reduced at the same time, and the uniformity of the epitaxial parameters can be improved, thereby improving the yield of the epitaxial wafer and the chip. This scheme adopts a wet or dry oxidation method to make the SiO2 insulating dielectric layer at the interface between the silicon substrate and the epitaxial. Compared with the ion implantation method, the damage to the lattice caused by the ion implantation process can be reduced. At the same time, since the wet and dry oxidation processes can batch process hundreds of substrates and form high-quality SiO2 layers, the ion implantation process requires single-chip processing, and when forming a certain thickness of insulating material, it is necessary to adjust the implantation energy for multiple implantations, and the subsequent annealing process repairs the lattice damage, so the processing method of this scheme has a lower cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is a schematic diagram of the epitaxial wafer structure of Example 1 of the present invention.

[0019] Figure 2a to Figure 2c This is a flow chart for epitaxial wafer production in Example 1.

[0020] Figure 3 This is a schematic diagram of the epitaxial wafer structure of Example 2 of the present invention.

[0021] Figures 4a to 4c This is a flow chart for epitaxial wafer production in Example 2.

[0022] Figure 5 This is a schematic diagram of the epitaxial wafer structure of Example 3 of the present invention.

[0023] Figures 6a to 6c This is the flow chart for epitaxial wafer production in Example 3.

[0024] Among them: 10-substrate; 11-quality layer; 12-transition layer; 13-buffer layer; 14-channel layer; 15-barrier layer; 20-substrate; 21-dielectric layer; 22-transition layer; 23-buffer layer; 24-channel layer; 25-barrier layer; 26-p-type GaN layer; 30-substrate; 31-dielectric layer; 32-transition layer; 33-buffer layer; 34-channel layer; 35-barrier layer 35; 36-SiN layer. DETAILED DESCRIPTION

[0025] The present disclosure will now be described more fully below with reference to the accompanying drawings, however, the present disclosure can be implemented in many different ways and should not be construed as being limited to the embodiments set forth herein. On the contrary, providing these embodiments herein will make the present disclosure more detailed and complete, and fully convey the scope of the present disclosure to those skilled in the art. The same reference numerals throughout the text represent the same objects.

[0026] Example 1

[0027] In a typical embodiment, the structure of the silicon substrate nitride semiconductor epitaxial wafer provided in this embodiment is as follows: Figure 1 As shown, it includes: a substrate 10, and a transition layer 12, a buffer layer 13, a channel layer 14, and a barrier layer 15 formed sequentially on the substrate 10. A silicon material with a certain thickness is converted into a SiO2 dielectric layer 11 between the substrate 10 and the transition layer 12 by a wet oxidation process.

[0028] In an optional embodiment, the substrate 10 is a silicon material substrate. The transition layer 12 is a 3C-SiC / AlN composite layer with a thickness of 0.1-200 nm.

[0029] In an optional embodiment, the buffer layer 13 is AlN, and the thickness of the buffer layer is generally 0.5-7 microns. However, the embodiments of the present disclosure are not limited thereto, and the buffer layer 13 may also be AlGaN, a GaN single layer or multilayer stacked structure, AlN / GaN, AlN / AlGaN, AlGaN / GaN superlattice structure, or a combination of the above structures.

[0030] In an optional embodiment, the channel layer 14 is made of GaN material with a thickness of 20-1000 nm. However, the embodiments of the present disclosure are not limited thereto, and the channel layer may also be made of AlGaN or InGaN material.

[0031] In an optional embodiment, the barrier layer 15 is an AlGaN layer with a thickness of 1-30 nm. However, the embodiments of the present disclosure are not limited thereto, and the barrier layer may also be an AlN layer, AlInN, or AlInGaN.

[0032] In an optional embodiment, an AlN insertion layer is further included below the barrier layer, with a thickness of 0.1-2 nm.

[0033] In an optional embodiment, the barrier layer may include a GaN cap layer with a thickness of 0.1-10 nm, or an in-situ SiN dielectric layer with a thickness of 0.5-150 nm, or a p-type GaN layer with a thickness of 10-200 nm.

[0034] The silicon substrate nitride semiconductor epitaxial wafer in the present disclosure is manufactured by the following steps:

[0035] Step 1, such as Figure 2a As shown, a silicon substrate 10 is provided, on which a transition layer 12 is grown. The growth process is metal organic chemical vapor deposition (MOCVD) or molecular beam epitaxy (MBE), or sputtering process, or other vapor deposition processes. In this embodiment, the transition layer includes a 10nm3C-SiC layer and an AlN nucleation layer grown thereon, with a thickness of 150nm.

[0036] Step 2, such as Figure 2b As shown, the epitaxial wafer after the transition layer 12 is grown is subjected to a wet oxidation process commonly used in silicon processing technology. Water vapor is introduced at high temperature to oxidize a silicon material layer of a certain thickness at the interface between the silicon substrate 10 and the transition layer 12 and transform it into a SiO2 insulating dielectric layer 11.

[0037] Step 3, such as Figure 2c As shown, after the SiO2 dielectric layer 11 is grown, a nitride buffer layer is grown on the epitaxial wafer, including a 100nm AlN layer, a 50nm AlGaN layer, and a 3000nm AlN / GaN superlattice structure. A 300nm GaN channel layer, a 1nm AlN insertion layer (not shown in the schematic diagram), and a 25nm AlGaN barrier layer are grown on the buffer layer.

[0038] Example 2

[0039] In the second exemplary embodiment, the structure of the silicon substrate nitride semiconductor epitaxial wafer is as follows Figure 3 As shown, it includes: a substrate 20, and a transition layer 22, a buffer layer 23, a channel layer 24, a barrier layer 25, and a p-type GaN layer 26 formed sequentially on the substrate 20. Between the substrate 20 and the transition layer 22, a silicon material with a certain thickness is converted into a SiO2 dielectric layer 21 through a dry oxidation process.

[0040] In an optional embodiment, the substrate 20 is a silicon material substrate, and the transition layer 22 is an AlN layer with a thickness of 0.1-200 nm.

[0041] In an optional embodiment, the buffer layer 23 is AlN with a thickness of 0.5-7 microns. However, the embodiments of the present disclosure are not limited thereto, and the buffer layer 23 may also be AlGaN, a GaN single layer or multilayer stacked structure, AlN / GaN, AlN / AlGaN, AlGaN / GaN superlattice structure, or a combination of the above structures.

[0042] In an optional embodiment, the channel layer 24 is made of GaN material with a thickness of 20-1000 nm. However, the embodiments of the present disclosure are not limited thereto, and the channel layer may also be made of AlGaN or InGaN material.

[0043] In an optional embodiment, the barrier layer 25 is an AlGaN layer with a thickness of 1-30 nm. However, the embodiments of the present disclosure are not limited thereto, and the barrier layer may also be a 25AlN layer, AlInN, AlInGaN, or a plurality of superpositions of the above material layers.

[0044] In an alternative embodiment, an AlN insertion layer is included below the barrier layer 25 with a thickness of 0.1-2 nm.

[0045] In an optional embodiment, the barrier layer 25 may include a GaN cap layer with a thickness of 0.1-10 nm, or an in-situ SiN dielectric layer with a thickness of 0.5-150 nm, or a p-type GaN layer with a thickness of 10-200 nm.

[0046] The silicon substrate nitride semiconductor epitaxial wafer in the present disclosure is manufactured by the following steps:

[0047] Step 1, such as Figure 4a As shown, a silicon substrate 20 is provided, on which a transition layer 22 is grown. The growth process is metal organic chemical vapor deposition (MOCVD) or molecular beam epitaxy (MBE), or sputtering process, or other vapor deposition process. In this embodiment, the transition layer includes an AlN nucleation layer grown by MOCVD process, with a thickness of 150nm.

[0048] Step 2, such as Figure 4b As shown, the epitaxial wafer after the transition layer 22 is grown is subjected to a dry oxidation process commonly used in silicon processing technology. O2 is introduced at high temperature to oxidize a silicon material layer of a certain thickness at the interface between the silicon substrate 20 and the transition layer 22, and transform it into a SiO2 insulating dielectric layer 21.

[0049] Step 3, such as Figure 4cAs shown, after the SiO2 dielectric layer 21 is grown, a nitride buffer layer is grown on the epitaxial wafer, including a 100nm AlN layer, a 50nm AlGaN layer, and a 3000nm AlN / GaN superlattice structure. A 300nm GaN channel layer, a 1nm AlN insertion layer (not shown in the schematic diagram), a 25nm AlGaN barrier layer, and an 80nm p-type GaN layer are grown on the buffer layer.

[0050] Example 3

[0051] In the third exemplary embodiment, the structure of the silicon substrate nitride semiconductor epitaxial wafer is as follows Figure 5 As shown, it includes: a substrate 30, and a transition layer 32, a buffer layer 33, a channel layer 34, a barrier layer 35, and an in-situ SiN layer 36 formed sequentially on the substrate 30. Between the substrate 30 and the transition layer 32, a silicon material with a certain thickness is transformed into a SiO2 dielectric layer 31 through a dry oxidation process.

[0052] In an optional embodiment, the substrate 30 is a silicon material substrate. The transition layer 32 is a 3C-SiC layer with a thickness of 0.1-200 nm.

[0053] In an optional embodiment, the buffer layer 33 is AlN with a thickness of 0.5-7 microns. However, the embodiments of the present disclosure are not limited thereto, and the buffer layer 33 may also be AlGaN, a GaN single layer or multilayer stacked structure, AlN / GaN, AlN / AlGaN, AlGaN / GaN superlattice structure, or a combination of the above structures.

[0054] In an optional embodiment, the channel layer 34 is made of GaN material with a thickness of 20-1000 nm. However, the embodiments of the present disclosure are not limited thereto, and the channel layer 34 may also be made of AlGaN or InGaN material.

[0055] In an optional embodiment, the barrier layer 35 is an AlGaN layer with a thickness of 1-30 nm. However, the embodiments of the present disclosure are not limited thereto, and the barrier layer 35 may also be an AlN layer, AlInN, AlInGaN, or a plurality of superpositions of the above material layers.

[0056] In an alternative embodiment, an AlN insertion layer is also included below the barrier layer, with a thickness of 0.1-2 nm.

[0057] In an optional embodiment, a GaN cap layer with a thickness of 0.1-10 nm, or an in-situ SiN dielectric layer with a thickness of 0.5-150 nm, or a p-type GaN layer with a thickness of 10-200 nm is included above the barrier layer.

[0058] The silicon substrate nitride semiconductor epitaxial wafer in the present disclosure is manufactured by the following steps:

[0059] Step 1, such as Figure 6a As shown, a silicon substrate 30 is provided, on which a transition layer 32 is grown. In this embodiment, the transition layer is a 3C-SiC single layer with a thickness of 20 nm.

[0060] Step 2, such as Figure 6b As shown, the epitaxial wafer after the transition layer 32 is grown is subjected to a dry oxidation process commonly used in silicon processing technology. O2 is introduced at high temperature to oxidize a silicon material layer of a certain thickness at the interface between the silicon substrate 30 and the transition layer 32, and transform it into a SiO2 insulating dielectric layer 31.

[0061] Step 3, such as Figure 6c As shown, after the SiO2 dielectric layer 31 is grown, a nitride buffer layer is grown on the epitaxial wafer, including a 100nm AlN layer, a 50nm AlGaN layer, and a 3000nm AlN / GaN superlattice structure. A 300nm GaN channel layer, a 1nm AlN insertion layer (not shown in the schematic diagram), a 25nm AlGaN barrier layer, and an 80nm in-situ SiN layer are grown on the buffer layer.

[0062] The above is only a specific implementation of the embodiment of the present invention, but the protection scope of the embodiment of the present invention is not limited thereto. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed in the embodiment of the present invention, which should be included in the protection scope of the embodiment of the present invention. Therefore, the protection scope of the embodiment of the present invention should be based on the protection scope of the claims.

Claims

1. An epitaxial preparation process, at least for preparing silicon substrate nitride semiconductor epitaxial, the structure of the silicon substrate nitride semiconductor epitaxial wafer at least includes: A silicon substrate and a transition layer formed on the silicon substrate, characterized in that the silicon material at the interface between the silicon substrate and the transition layer is oxidized or nitrided to form an insulating dielectric layer.

2. An epitaxial preparation process according to claim 1, characterized in that: A buffer layer, a channel layer and a barrier layer are arranged in sequence above the transition layer.

3. An epitaxial preparation process according to claim 1, characterized in that: The transition layer is selected from one of the following materials: gallium nitride, aluminum nitride, indium nitride, or alloy materials or multi-layer stacked structures of the above materials; or 3C-SiC material, SiN material; or first growing a layer of 3C-SiC or SiN material on the surface of the silicon substrate, and then continuing to grow the above gallium nitride, aluminum nitride, indium nitride, or alloy materials or multi-layer stacked structures of the above materials.

4. An epitaxial preparation process according to claim 1, characterized in that: The oxidation process is selected from one of the following processes: dry oxidation process, wet oxidation process.

5. An epitaxial preparation process according to claim 1, characterized in that: The nitriding process is selected from one of the following processes: Treating the substrate using a nitrogen-containing gas in a high temperature environment; The substrate is exposed to a plasma atmosphere containing N element.

6. An epitaxial preparation process according to claim 1, characterized in that: The buffer layer is made of one of the following materials: AlN, AlGaN, GaN single layer or multi-layer stacked structure, AlN / GaN, AlN / AlGaN, AlGaN / GaN super lattice structure, or a combination of the above structures.

7. An epitaxial preparation process according to claim 1, characterized in that: The channel layer is selected from one of the following materials: GaN material, AlGaN material, and InGaN material.

8. An epitaxial preparation process according to claim 1, characterized in that: The barrier layer is selected from one of the following materials: AlGaN layer, AlN layer, AlInN, AlInGaN, and a plurality of superpositions of the above material layers.

9. An epitaxial preparation process according to claim 1, characterized in that: An AlN insertion layer is included between the channel layer and the barrier layer.

10. The epitaxial preparation process according to claim 1, characterized in that: At least one of the following is included above the barrier layer: an unintentionally doped GaN cap layer, an in-situ SiN dielectric layer, and a p-type AlGaInN alloy layer of any proportion.

Citation Information

Cited By

  • Composite substrate nitride epitaxial wafer and preparation method thereof

    CN120690672A