Method for repairing integrity of sealing surface of aluminum alloy shell

Through cold spraying technology combined with deep cold ironing technology, the performance degradation caused by stress corrosion of the sealing surface of aluminum alloy shell is solved, and the surface hardness and integrity are significantly improved, which extends the service life of the parts and saves economic costs. .

CN118926824AActive Publication Date: 2024-11-12WUHU STATE-OWNED FACTORY OF MACHINING

Patent Information

Application Number
CN202410966877.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-12
Estimated Expiration
2044-07-18

AI Technical Summary

Technical Problem

The sealing surface of aluminum alloy shells produces fine cracks and corrosion pits due to stress corrosion, resulting in a decrease in sealing performance. The existing welding and cold spray repair processes have low adaptability, large heat output, pores, cracks, inclusions and coating surface hardness. The problem of low affects the sealing performance.

Method used

Using cold spraying technology combined with deep cold ironing technology, the sealing surface of aluminum alloy shell is significantly improved through decomposition and cleaning, surface grinding, deep cold ironing, sandblasting, preheating, spraying and secondary deep cold ironing. Hardness and integrity reduce surface roughness and ensure sealing performance.

Benefits of technology

Effectively avoid the heat input problem of welding process and the loose coating and low hardness of the cold spray process, realize deep repair of surface defects, significantly improve the integrity and hardness of the sealing surface, extend the service life of the parts, and reduce the Scrap and replacement costs of parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118926824A_ABST
    Figure CN118926824A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of remanufacturing, in particular to an aluminum alloy shell sealing surface integrity repairing method which comprises the following steps: (1) decomposing and cleaning; (2) grinding the surface; (3) primary cryogenic ironing treatment; (4) primary dye penetrant inspection; (5) protecting the parts; (6) cleaning; (7) surface pretreatment; (8) preheating before spraying; (10) processing after coating; (11) secondary cryogenic ironing treatment; and (12) secondary dye penetrant inspection. According to the method, the problems that a traditional welding process is large in heat input, air holes, cracks and inclusions are prone to being generated or local hardness is not matched are effectively solved, and the problems that a conventional cold spraying repairing coating is loose, prone to chipping and low in surface hardness, and the surface roughness of the coating depends on machining are also effectively solved. Effective repair of the shell sealing surface defect depth from several micrometers to several millimeters is achieved, the surface roughness of a repaired part is remarkably reduced, the surface hardness is remarkably improved, and the coating density is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of remanufacturing, and in particular to a method for repairing the integrity of a sealing surface of an aluminum alloy housing. Background Art

[0002] Aluminum alloy has the advantages of low density, high specific strength, good corrosion resistance, and easy processing, and has been widely used in the aerospace field. Cast aluminum alloy is widely used in various parts and accessories in aircraft fuel and hydraulic systems. However, the oil environment is often corrosive. When the shell parts have been in service for a long time, the shell sealing surface will produce small cracks and corrosion pits on the surface due to stress corrosion, affecting the sealing performance.

[0003] At present, welding or conventional cold spraying is mostly used to restore the sealing surface function of such parts. However, welding repair methods have problems such as low compatibility between the repair layer and the base material, large heat output, easy to produce defects such as pores, cracks, inclusions, or local hardness mismatch, which in turn affects the sealing performance; conventional cold spray repair methods will have problems such as loose and porous coating surface, coating surface roughness relying on machining methods, and low coating surface hardness. The sealing performance of parts cannot be guaranteed after long-term work. In response to the above problems, this paper proposes a method for repairing the integrity of the sealing surface of an aluminum alloy shell, using a cold spraying process to achieve surface additive material restoration, and combining deep cold ironing technology to significantly improve the hardness of the sealing surface of the aluminum alloy shell, reduce the surface roughness, and improve the surface integrity, thereby restoring the sealing performance of the shell surface and greatly extending the service life of the aluminum alloy shell. Summary of the invention

[0004] In order to solve the above technical problems, the present invention proposes a method for repairing the integrity of the sealing surface of an aluminum alloy housing, which makes up for the defects of existing welding and cold spraying repair processes, solves the problem of aluminum alloy housing parts being scrapped due to insufficient repair means after the sealing surface is damaged, improves the repair success rate of parts, reduces the replacement of parts and accessories, and greatly saves costs.

[0005] The technical problem to be solved by the present invention is achieved by adopting the following technical solutions:

[0006] A method for repairing the integrity of the sealing surface of an aluminum alloy housing comprises the following steps:

[0007] (1) Decomposition and cleaning: Decompose the redundant structures on the aluminum alloy shell into the smallest repair unit that cannot be decomposed, and then use an organic solvent to clean the aluminum alloy shell after decomposition;

[0008] (2) Surface grinding: Use machining to remove surface defects of the aluminum alloy housing seal until a defect-free surface is obtained;

[0009] (3) Primary cryogenic ironing treatment: A diamond elastic tool is used and the primary cryogenic ironing process parameters are set to perform the ironing treatment on the sealing surface of the aluminum alloy housing. During the ironing treatment, liquid nitrogen is continuously poured at a flow rate of 0.1 to 0.3 L / min to provide a low-temperature environment and lubricating oil is injected for surface lubrication;

[0010] The process parameters of a deep cold ironing are as follows:

[0011] The ironing depth is 0.025-0.035mm, the tool moving speed is 10-100mm / s, the ironing step is 0.005-0.010mm, and the ironing passes are 2-4 times;

[0012] (4) Primary color penetration testing: Use the color penetration method to test the defective polished area to ensure that the defect is completely eliminated. If there is a defect, repeat steps (2) to (3) until the defect is completely eliminated.

[0013] (5) Parts protection: Use high temperature masking tape and high temperature resistant glue to seal and protect the aluminum alloy shell;

[0014] (6) Cleaning: Clean the area of ​​the aluminum alloy shell to be sprayed with an organic solvent and wipe it with a clean, lint-free cotton cloth. After wiping, blow dry the surface of the part with clean, dry compressed air;

[0015] (7) Surface pretreatment: For the area of ​​the aluminum alloy shell to be sprayed, use 40-60 mesh brown corundum sand and set the sandblasting process parameters for sandblasting. After spraying, use clean and dry compressed air to blow away the remaining sand particles. The surface of the part after sandblasting should be rough and uniform, without gloss and dark spots, and the roughness Ra5.0-7.6μm;

[0016] The sandblasting process parameters are as follows:

[0017] The sandblasting pressure is 0.25-0.35MPa, the sandblasting distance is 150-200mm, the sandblasting gun is not allowed to stay on the aluminum alloy shell for more than 15s, and the sandblasting area completely covers the surface to be repaired;

[0018] (8) Preheating before spraying: Use oven heating method and preheat at a temperature of 60-70°C;

[0019] (9) Parts spraying: Use cold spraying process and set cold spraying process parameters for additive manufacturing. During the spraying process, the temperature of the aluminum alloy shell substrate is controlled below 120°C. The spraying process must be continuous, and the spraying pause time must not exceed 10 minutes. During spraying and spraying pauses, use compressed air to cool the aluminum alloy shell;

[0020] The cold spraying process parameters are as follows:

[0021] The coating material is aluminum + 30% alumina powder, 2024 aluminum alloy powder or 2024 aluminum alloy + 30% alumina powder, the powder particle size is 15-53μm, the spraying carrier gas is compressed air or nitrogen, the distance between the spray gun outlet and the surface to be sprayed is 10-25mm, the spray gun pressure is 1-1.5MPa, the heating temperature is 350-500℃, and the powder feeding amount is 15-35g / min;

[0022] (10) Post-coating processing: According to the repair position of the aluminum alloy shell and the dimensional accuracy requirements of the pattern, mechanical grinding can be used for processing. The coating should be smooth after grinding, without edges and corners, and the roughness should not be inferior to Ra3.2μm;

[0023] (11) Secondary cryogenic ironing treatment: A diamond elastic tool is used and secondary cryogenic ironing process parameters are set to perform ironing treatment on the sealing surface of the aluminum alloy housing. During the ironing treatment, liquid nitrogen is continuously poured at a flow rate of 0.1 to 0.3 L / min to provide a low-temperature environment and lubricating oil is injected for surface lubrication;

[0024] The process parameters of secondary deep cold ironing are as follows:

[0025] The ironing depth is 0.005-0.035mm, the tool moving speed is 10-100mm / s, the ironing step is 0.005-0.010mm, and the ironing passes are 2-4 times;

[0026] (12) Secondary color flaw detection: The coating surface after the secondary deep cold ironing treatment is subjected to color flaw detection. It is required that there are no cracks in the surface reinforcement area and transition area of ​​the part. If there are defects, the process (2) to (11) is repeated until the flaw detection is qualified.

[0027] As a further improvement of the present invention, the organic solvent in step (1) includes aviation organic solvent and acetone.

[0028] As a further improvement of the present invention, the defects in step (2) include cracks and corrosion pits.

[0029] As a further improvement of the present invention, in step (5), the holes and cavities on the aluminum alloy shell are protected.

[0030] As a further improvement of the present invention, the organic solvent in step (6) includes alcohol and acetone.

[0031] As a further improvement of the present invention, the interval between step (6) and step (9) shall not exceed 4 hours.

[0032] As a further improvement of the present invention, the interval between step (7) and step (9) shall not exceed 2 hours.

[0033] As a further improvement of the present invention, the temperature is required to be monitored during the preheating process in step (8).

[0034] As a further improvement of the present invention, the coating after spraying in step (9) has a processing allowance of 1 to 2 mm.

[0035] The beneficial effects of the present invention are:

[0036] The present invention provides a method for repairing the integrity of the sealing surface of an aluminum alloy shell, which effectively avoids the problems of large heat input, easy generation of pores, cracks, inclusions or local hardness mismatch in traditional welding processes, and also effectively solves the problems of loose and easy falling of conventional cold spray repair coatings, low surface hardness, and reliance on machining for coating surface roughness. The present invention can effectively repair surface defects of the shell seal with a depth of several microns to several millimeters at an operating temperature below 120°C. The surface roughness of the repaired parts is significantly reduced, the surface hardness is significantly improved, and the density of the coating is greatly improved, thereby greatly improving the surface integrity of the shell sealing surface, thereby reducing the scrapping of parts due to insufficient repair means and saving economic costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] The present invention is further described below in conjunction with the accompanying drawings and embodiments:

[0038] Figure 1 It is a flow chart of the present invention. DETAILED DESCRIPTION

[0039] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below with reference to the accompanying drawings and embodiments.

[0040] like Figure 1 As shown, a method for repairing the integrity of the sealing surface of an aluminum alloy housing comprises the following steps:

[0041] (1) Decomposition and cleaning: Decompose the redundant structures on the aluminum alloy shell into the smallest indecomposable repair unit. After decomposition, use aviation organic solvents, acetone and other organic solvents to clean the aluminum alloy shell to avoid residual fuel in the internal pipes and inner holes of the shell that affect subsequent repairs.

[0042] (2) Surface grinding: Use machining to remove surface defects of the aluminum alloy housing seal until a defect-free surface is obtained.

[0043] (3) Primary cryogenic ironing treatment: A diamond elastic tool is used and the primary cryogenic ironing process parameters are set to perform the ironing treatment on the sealing surface of the aluminum alloy housing. During the ironing treatment, liquid nitrogen is continuously poured at a flow rate of 0.1 to 0.3 L / min to provide a low-temperature environment and lubricating oil is injected for surface lubrication;

[0044] The process parameters of a deep cold ironing are as follows:

[0045] The ironing depth is 0.025-0.035 mm, the tool moving speed is 10-100 mm / s, the ironing step is 0.005-0.010 mm, and the ironing passes are 2-4 times.

[0046] In this embodiment, the flow rate of pouring liquid nitrogen is specifically controlled at 0.1L / min, and the process parameters of a deep cold ironing are specifically as follows: the ironing depth is 0.035mm, the tool moving speed is 100mm / s, the ironing step is 0.010mm, and the ironing passes are 4 times.

[0047] (4) Primary color penetration inspection: Use the color penetration method to inspect the defective polished area to ensure that the defect is completely eliminated. If there is a defect, repeat steps (2) to (3) until the defect is completely eliminated.

[0048] (5) Parts protection: Use high-temperature masking tape and high-temperature resistant glue to seal and protect the aluminum alloy shell, focusing on protecting the holes, cavities and other parts on the aluminum alloy shell to prevent sand and dust from entering the interior.

[0049] (6) Cleaning: Clean the area of ​​the aluminum alloy shell to be sprayed with an organic solvent and wipe it with a clean, lint-free cotton cloth. After wiping, blow dry the surface of the part with clean, dry compressed air. The time interval between the last cleaning and spraying should not exceed 4 hours.

[0050] (7) Surface pretreatment: For the area of ​​the aluminum alloy shell to be sprayed, use 40-60 mesh brown corundum sand and set the sandblasting process parameters for sandblasting. After spraying, use clean and dry compressed air to blow away the remaining sand particles. The surface of the part after sandblasting should be rough and uniform, without gloss and dark spots, and the roughness Ra5.0-7.6μm;

[0051] The sandblasting process parameters are as follows:

[0052] The sandblasting pressure is 0.25-0.35MPa, the sandblasting distance is 150-200mm, the sandblasting gun is not allowed to stay on the aluminum alloy shell for more than 15s, and the sandblasting area completely covers the surface to be repaired.

[0053] In this embodiment, 60-mesh brown corundum sand is specifically used, and the sandblasting pressure is specifically 0.25 MPa, the sandblasting distance is 200 mm, and the roughness Ra after sandblasting is specifically 7.6 μm.

[0054] (8) Preheating before spraying: Use oven heating method and preheat at a temperature of 60-70°C. During the preheating process, the temperature needs to be monitored to avoid overheating.

[0055] In this embodiment, the preheating temperature is specifically 70°C.

[0056] (9) Parts spraying: Use cold spraying process and set cold spraying process parameters for additive manufacturing. During the spraying process, the temperature of the aluminum alloy shell substrate is controlled below 120°C. The spraying process must be continuous, and the spraying pause time must not exceed 10 minutes. During spraying and spraying pauses, use compressed air to cool the aluminum alloy shell;

[0057] The cold spraying process parameters are as follows:

[0058] The coating material is aluminum + 30% alumina powder, 2024 aluminum alloy powder or 2024 aluminum alloy + 30% alumina powder, the powder particle size is 15-53μm, the spray carrier gas is compressed air or nitrogen, the distance between the spray gun outlet and the surface to be sprayed is 10-25mm, the spray gun pressure is 1-1.5MPa, the heating temperature is 350-500℃, and the powder feeding amount is 15-35g / min.

[0059] In this embodiment, the coating material is specifically 2024 aluminum alloy + 30% alumina powder, the powder particle size is 53μm, the spray carrier gas is compressed air, the distance between the spray gun outlet and the surface to be sprayed is 25mm, the spray gun pressure is 1.5MPa, the heating temperature is 350℃, and the powder feeding amount is 35g / min.

[0060] (10) Post-coating processing: According to the repair position of the aluminum alloy shell and the dimensional accuracy requirements of the pattern, mechanical grinding can be used for processing. If there are no special requirements, the coating is required to have a smooth transition after grinding, without edges and corners, and the roughness is not inferior to Ra3.2μm.

[0061] (11) Secondary cryogenic ironing treatment: A diamond elastic tool is used and secondary cryogenic ironing process parameters are set to perform ironing treatment on the sealing surface of the aluminum alloy housing. During the ironing treatment, liquid nitrogen is continuously poured at a flow rate of 0.1 to 0.3 L / min to provide a low-temperature environment and lubricating oil is injected for surface lubrication;

[0062] The process parameters of secondary deep cold ironing are as follows:

[0063] The ironing depth is 0.005-0.035 mm, the tool moving speed is 10-100 mm / s, the ironing step is 0.005-0.010 mm, and the ironing passes are 2-4 times.

[0064] In this embodiment, the flow rate of pouring liquid nitrogen is specifically controlled at 0.3L / min, and the secondary deep cold ironing process parameters are specifically as follows: ironing depth is 0.035mm, tool moving speed is 10mm / s, ironing step is 0.005mm, and ironing pass is 2 times.

[0065] (12) Secondary color flaw detection: The coating surface after the secondary deep cold ironing treatment is subjected to color flaw detection. It is required that there are no cracks in the surface reinforcement area and transition area of ​​the part. If there are defects, the process (2) to (11) is repeated until the flaw detection is qualified.

[0066] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions only describe the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for repairing the integrity of the sealing surface of an aluminum alloy housing, characterized in that: The following steps are involved: (1) Decomposition and cleaning: Decompose the redundant structures on the aluminum alloy shell into the smallest repair unit that cannot be decomposed, and then use an organic solvent to clean the aluminum alloy shell after decomposition; (2) Surface grinding: Use machining to remove surface defects of the aluminum alloy housing seal until a defect-free surface is obtained; (3) Primary cryogenic ironing treatment: A diamond elastic tool is used and the primary cryogenic ironing process parameters are set to perform the ironing treatment on the sealing surface of the aluminum alloy housing. During the ironing treatment, liquid nitrogen is continuously poured at a flow rate of 0.1 to 0.3 L / min to provide a low-temperature environment and lubricating oil is injected for surface lubrication; The process parameters of a deep cold ironing are as follows: The ironing depth is 0.025-0.035mm, the tool moving speed is 10-100mm / s, the ironing step is 0.005-0.010mm, and the ironing passes are 2-4 times; (4) Primary color penetration testing: Use the color penetration method to test the defective polished area to ensure that the defect is completely eliminated. If there is a defect, repeat steps (2) to (3) until the defect is completely eliminated. (5) Parts protection: Use high temperature masking tape and high temperature resistant glue to seal and protect the aluminum alloy shell; (6) Cleaning: Clean the area of ​​the aluminum alloy shell to be sprayed with an organic solvent and wipe it with a clean, lint-free cotton cloth. After wiping, blow dry the surface of the part with clean, dry compressed air; (7) Surface pretreatment: For the area of ​​the aluminum alloy shell to be sprayed, use 40-60 mesh brown corundum sand and set the sandblasting process parameters for sandblasting. After spraying, use clean and dry compressed air to blow away the remaining sand particles. The surface of the part after sandblasting should be rough and uniform, without gloss and dark spots, and the roughness Ra5.0-7.6μm; The sandblasting process parameters are as follows: The sandblasting pressure is 0.25-0.35MPa, the sandblasting distance is 150-200mm, the sandblasting gun is not allowed to stay on the aluminum alloy shell for more than 15s, and the sandblasting area completely covers the surface to be repaired; (8) Preheating before spraying: Use oven heating method and preheat at a temperature of 60-70°C; (9) Parts spraying: Use cold spraying process and set cold spraying process parameters for additive manufacturing. During the spraying process, the temperature of the aluminum alloy shell substrate is controlled below 120°C. The spraying process must be continuous, and the spraying pause time must not exceed 10 minutes. During spraying and spraying pauses, use compressed air to cool the aluminum alloy shell; The cold spraying process parameters are as follows: The coating material is aluminum + 30% alumina powder, 2024 aluminum alloy powder or 2024 aluminum alloy + 30% alumina powder, the powder particle size is 15-53μm, the spraying carrier gas is compressed air or nitrogen, the distance between the spray gun outlet and the surface to be sprayed is 10-25mm, the spray gun pressure is 1-1.5MPa, the heating temperature is 350-500℃, and the powder feeding amount is 15-35g / min; (10) Post-coating processing: According to the repair position of the aluminum alloy shell and the dimensional accuracy requirements of the pattern, mechanical grinding can be used for processing. The coating should be smooth after grinding, without edges and corners, and the roughness should not be inferior to Ra3.2μm; (11) Secondary cryogenic ironing treatment: A diamond elastic tool is used and secondary cryogenic ironing process parameters are set to perform ironing treatment on the sealing surface of the aluminum alloy housing. During the ironing treatment, liquid nitrogen is continuously poured at a flow rate of 0.1 to 0.3 L / min to provide a low-temperature environment and lubricating oil is injected for surface lubrication; The process parameters of secondary deep cold ironing are as follows: The ironing depth is 0.005-0.035mm, the tool moving speed is 10-100mm / s, the ironing step is 0.005-0.010mm, and the ironing passes are 2-4 times; (12) Secondary color flaw detection: The coating surface after the secondary deep cold ironing treatment is subjected to color flaw detection. It is required that there are no cracks in the surface reinforcement area and transition area of ​​the part. If there are defects, the process (2) to (11) is repeated until the flaw detection is qualified.

2. The method for repairing the integrity of the sealing surface of an aluminum alloy housing according to claim 1, characterized in that: The organic solvent in step (1) includes aviation organic solvent and acetone.

3. The method for repairing the integrity of the sealing surface of an aluminum alloy housing according to claim 1, characterized in that: Defects in process (2) include cracks and corrosion pits.

4. The method for repairing the integrity of the sealing surface of an aluminum alloy housing according to claim 1, characterized in that: In step (5), the focus is on protecting the holes and cavities on the aluminum alloy shell.

5. The method for repairing the integrity of the sealing surface of an aluminum alloy housing according to claim 1, characterized in that: The organic solvent in step (6) includes alcohol and acetone.

6. The method for repairing the integrity of the sealing surface of an aluminum alloy housing according to claim 1, characterized in that: The interval between step (6) and step (9) shall not exceed 4 hours.

7. The method for repairing the integrity of the sealing surface of an aluminum alloy housing according to claim 1, characterized in that: The interval between step (7) and step (9) shall not exceed 2 hours.

8. The method for repairing the integrity of the sealing surface of an aluminum alloy housing according to claim 1, characterized in that: During the preheating process in step (8), the temperature must be monitored.

9. The method for repairing the integrity of the sealing surface of an aluminum alloy housing according to claim 1, characterized in that: The coating after spraying in step (9) has a processing allowance of 1 to 2 mm.

Citation Information

Patent Citations

  • Method for intensifying laser cladding layer through ultrasonic rolling

    CN107400887A

  • Composite material and preparation method thereof

    CN109929986A

  • Remanufacturing and repairing technology for piston rod with non-degradable sealing ring for aircraft

    CN110408879A

  • Method for repairing aircraft fuel system aluminum silicon alloy shell casting defects

    CN110480254A

  • Anti-deformation repairing method for thin-wall shell of aircraft control handle

    CN111996523A

Cited By

  • Method for repairing aero aluminum alloy parts and high-entropy composite coating

    CN122727780A