High-purity spherical titanium dioxide and preparation method thereof

Through acidolysis, hydrothermal reaction and roasting, combined with the use of citric acid and sodium dodecylbenzenesulfonate, as well as polysuccinimide derivative dispersant, the problem of impurity adsorption in the wet process is solved, and the problem of impurity adsorption in the wet process is achieved The preparation of high-purity spherical titanium dioxide improves resource utilization efficiency and purity, and solves the problems of resource waste and environmental pollution.

CN118929745AActive Publication Date: 2024-11-12HUBEI ZHANPENG ELECTRONIC MATERIALS CO LTD

Patent Information

Application Number
CN202411065396.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-12
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

In the existing wet process, the hydrolyzed partial titanium acid obtained by hydrolysis after acid dissolution of titanium-containing blast furnace slag acid is large, which is very easy to adsorb impurity ions such as ferrous, affecting the purity of titanium dioxide. Moreover, the titanium content in domestic titanium-containing blast furnace slag is relatively high. , cannot be used directly as building materials, resulting in waste of resources and environmental pollution.

Method used

Using acidolysis, hydrothermal reaction, desulfurization and roasting, citric acid and sodium dodecylbenzenesulfonate to remove impurities, and the dispersion of metatitanic acid is adjusted through polysuccinimide derivative dispersant to form a high Pure spherical titanium dioxide.

Benefits of technology

Effectively remove impurities, improve the purity and economic benefits of titanium dioxide, realize the resource utilization of industrial waste, reduce the impurity ion content and aggregation of metatitanic acid, and improve dispersion stability and spherical shape.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929745A_ABST
    Figure CN118929745A_ABST
Patent Text Reader

Abstract

The invention discloses high-purity spherical titanium dioxide and a preparation method thereof. The preparation method comprises the following steps: firstly, crushing titanium-containing blast furnace slag, grinding and sieving; then mixing with a sulfuric acid solution and an additive, heating and reacting to obtain an impurity-containing titanyl sulfate solution; then adding a polysuccinimide derivative and carrying out hydrothermal reaction to obtain hydrothermal metatitanic acid; mixing the metatitanic acid with a NaOH solution to prepare slurry, and filtering, washing and drying after reaction to obtain desulfurized metatitanic acid; and finally roasting and cooling to obtain the catalyst. According to the method, the titanium-containing blast furnace slag is used as the raw material, the complexing agent, the surface active agent and the dispersing agent are adopted in the technological process, impurities are effectively removed, the high-purity spherical titanium dioxide product is obtained, resource utilization of industrial waste is achieved, economic benefits are improved, and the method has remarkable technical value and application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of titanium dioxide preparation, and in particular to high-purity spherical titanium dioxide and a preparation method thereof. Background Art

[0002] Titanium resources are important strategic resources and are widely used in many production fields such as coatings, plastics, papermaking, and printing inks. my country is a country with abundant titanium resources, and its reserves of titanium rank first in the world. my country's titanium resources are mainly distributed in Panzhihua and Chengde. The reserves of vanadium-titanium magnetite in Panzhihua exceed 9 billion tons. During the smelting process, a large amount of titanium-containing blast furnace slag is produced as a by-product. The Panxi region produces more than 7 million tons of titanium-containing blast furnace slag each year. Compared with titanium-rich ore, the titanium content in titanium-containing blast furnace slag is low and cannot be directly used as a raw material for the preparation of high-grade titanium dioxide. Although studies have shown that the addition of an appropriate amount of blast furnace slag is beneficial to enhancing the mechanical properties of building materials. However, when the titanium content in blast furnace slag exceeds 10%, the strength of the building material will decrease. The titanium dioxide content in foreign titanium-containing blast furnace slag is usually no more than 10%, which can be directly used as a building material, while the titanium content in domestic titanium-containing blast furnace slag is high and cannot be directly used as a building material. The difficulty in large-scale resource utilization has led to a large accumulation of titanium-containing blast furnace slag, causing waste of land resources and environmental pollution, as well as waste of valuable elements such as titanium and aluminum. Therefore, the recovery and resource utilization of valuable elements in titanium-containing blast furnace slag, especially titanium, has attracted widespread attention in China.

[0003] The titanium-containing blast furnace slag has a complex ore phase, contains a large amount of complex silicates, and the titanium-containing mineral grains are fine, mainly in a complex crystal structure, and it is difficult to improve its grade through effective ore dressing. Over the past few decades, many scholars have conducted extensive research on it, which can be roughly divided into pyrometallurgical processes and hydrometallurgical processes. The hydrometallurgical process mainly uses alkaline leaching or acid hydrolysis, and the acid hydrolysis agents commonly used are sulfuric acid and hydrochloric acid.

[0004] Chinese patent document CN114014359A discloses a method for extracting titanium dioxide from titanium-containing blast furnace slag, comprising the following steps: A. drying the titanium-containing blast furnace slag and grinding it into powder to obtain blast furnace slag powder; B. adding sulfuric acid to the blast furnace slag powder and stirring it evenly, then adding hydrogen peroxide and letting it stand and soak to obtain a soaked mixture; C. separating the soaked mixture from solid and liquid, and washing the solid phase with hydrogen peroxide to obtain a hydrogen peroxide complex liquid; D. decomposing the hydrogen peroxide complex liquid to obtain titanium dioxide.

[0005] In the existing wet process, the hydrolyzed titanic acid obtained by acid hydrolysis of titanium-containing blast furnace slag has a large specific surface area and colloidal properties. It is very easy to adsorb impurity ions such as ferrous iron and carry them out with the titanic acid, affecting the purity of the final TiO2 product. Summary of the invention

[0006] In order to solve the shortcomings of the prior art, the purpose of the present invention is to provide a high-purity spherical titanium dioxide and a preparation method thereof, using titanium-containing blast furnace slag as raw material, and effectively removing impurities through acid hydrolysis, hydrothermal reaction, desulfurization and roasting, etc., to finally obtain a high-purity titanium dioxide product, thereby realizing the resource utilization of industrial waste and improving economic benefits, and having significant technical value and application prospects.

[0007] In order to achieve the above object, the present invention adopts the following technical solution:

[0008] A method for preparing high-purity spherical titanium dioxide comprises the following steps:

[0009] (1) crushing, grinding and sieving titanium-containing blast furnace slag;

[0010] (2) mixing the sieved titanium-containing blast furnace slag with a sulfuric acid solution, adding citric acid and sodium dodecylbenzene sulfonate, heating for reaction, and obtaining an acid hydrolysis slag; adding the acid hydrolysis slag into deionized water, stirring and mixing, and filtering to obtain an impure sulfuric acid-containing titanium oxide solution;

[0011] (3) adding the titanium dioxide solution containing the impurity sulfate and the polysuccinimide derivative into a reaction kettle, sealing the reaction kettle, cooling the product, filtering the product to obtain a filter cake, washing the filter cake, and drying the filter cake to obtain hydrothermal metatitanic acid;

[0012] (4) Mixing hydrothermal metatitanic acid and NaOH solution to form a slurry, adjusting the pH, stirring at room temperature, filtering, washing, and drying the product to obtain desulfurized metatitanic acid; calcining the desulfurized metatitanic acid, and cooling to obtain the high-purity spherical titanium dioxide.

[0013] Preferably, in step (1), the product is sieved through a 200-600 mesh sieve.

[0014] Preferably, in step (2), the concentration of the sulfuric acid solution is 85-98wt%; the heating reaction conditions are 70-130°C for 1-6h; the dosage ratio of the titanium-containing blast furnace slag to the sulfuric acid solution is 1:1.5-2.2; the dosage of citric acid and sodium dodecylbenzene sulfonate is 0.01-0.5wt% and 0.5-2wt% of the titanium-containing blast furnace slag, respectively; and the dosage ratio of the acid hydrolysis slag to deionized water is 1:1-2.

[0015] Preferably, in step (3), the sealed reaction conditions are hydrothermal reaction at 110-160° C. and 0.2-1 MPa for 1-12 hours; the mass ratio of the heterosulfate-containing titanyl solution to the polysuccinimide derivative is 100:0.1-3.

[0016] Preferably, in step (4), the concentration of NaOH solution is 0.5-5wt%, and the pH is adjusted to 10-14; the stirring conditions at room temperature are stirring at 400-800r / min for 30-120min, the drying conditions are drying at 100-110°C for 1-3h; and the calcination conditions are calcining in a muffle furnace at 500-1000°C for 2-5h.

[0017] Specifically, the structural formula of the polysuccinimide derivative is as follows:

[0018]

[0019] Preferably, the preparation method of the polysuccinimide derivative comprises the following steps:

[0020] a. Dissolve polysuccinimide in DMSO to obtain a PSI solution; dissolve dopamine hydrochloride in DMSO, then add triethylamine, and ultrasonically oscillate to obtain a dopamine solution; add the dopamine solution to the PSI solution, and reflux under a nitrogen atmosphere to obtain a PSI-DA intermediate reaction solution;

[0021] Preferably, in step a, the dosage ratio of PSI, dopamine hydrochloride and triethylamine is 40mmol:10-15mmol:8-16mL; the ultrasonic oscillation time is 10-30min; and the reflux reaction conditions are reflux reaction at 50-70°C for 18-30h.

[0022] b. Dissolve glutamic acid in DMSO, then add triethylamine, and ultrasonically oscillate to obtain a glutamic acid solution; add the glutamic acid solution to the reaction solution obtained in step (1), stir the reaction under a nitrogen atmosphere, adjust the pH with an aqueous sodium hydroxide solution, precipitate the product with acetone, filter, wash with acetone, and dry to obtain the polysuccinimide derivative.

[0023] Preferably, in step b, the ratio of glutamic acid to triethylamine is 30 mmol:10-20 mL; the stirring reaction conditions are stirring the reaction at 50-70° C. for 12-20 h, and after the reaction is completed, the pH is adjusted to 7-8.

[0024] Preferably, the molar ratio of polysuccinimide, dopamine hydrochloride and glutamic acid is 40:10-15:30-25.

[0025] The reaction involves two major steps, first the reaction of polysuccinimide (PSI) with dopamine (DA), and then the reaction of the PSI-DA intermediate with glutamic acid. In the first step, triethylamine acts as a strong base to neutralize dopamine hydrochloride, releasing free dopamine. The primary amine group (-NH2) of dopamine then undergoes nucleophilic addition to the imide ring of PSI. This process involves the nitrogen atom of the amino group attacking the carbonyl carbon of the imide ring to form a tetrahedral intermediate, which then collapses, leading to the opening of the imide ring and ultimately grafting dopamine onto the polysuccinimide molecular chain.

[0026] In the second step, the α-amino group of glutamic acid undergoes a similar nucleophilic addition reaction to the remaining PSI imide ring. This process is similar to the first step, and also includes the amino group attacking the carbonyl carbon of the imide ring to form a tetrahedral intermediate, the intermediate collapses, the imide ring opens, and glutamic acid is grafted onto the polysuccinimide molecule.

[0027] The result of the whole reaction is that part of the imide rings on the PSI main chain are opened by dopamine, and dopamine side chains are introduced, and the remaining imide rings are opened by glutamic acid, and glutamic acid side chains are introduced. The final product is a polymer containing dopamine and glutamic acid side chains, and some unreacted imide rings may remain on the main chain.

[0028] By introducing side chains with specific functions onto the PSI skeleton, an amphiphilic polymer with good dispersion properties was successfully synthesized. It also combined multiple action mechanisms such as electrostatic stabilization, stereo stabilization and chemical adsorption to achieve an efficient and stable dispersion effect.

[0029] The present invention also claims to protect high-purity spherical titanium dioxide prepared by the preparation method.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] 1) The present invention provides a method for preparing high-purity spherical titanium dioxide, which uses titanium-containing blast furnace slag as a raw material, effectively removes impurities through acidolysis, hydrothermal reaction, desulfurization and roasting, and finally obtains a high-purity titanium dioxide product, realizes the resource utilization of industrial waste, improves economic benefits, and has significant technical value and application prospects. In terms of process optimization, the addition of citric acid and sodium dodecylbenzene sulfonate significantly reduces the content of impurity ions and improves the acidolysis efficiency, while the use of a polysuccinimide derivative dispersant reduces the agglomeration during the hydrolysis of metatitanic acid, which is conducive to the subsequent formation of titanium dioxide with good dispersibility and sphericity.

[0032] 2) The present invention provides a polysuccinimide derivative dispersant, wherein the glutamic acid side chain contains a large number of carboxylic acid groups, which form carboxylates under alkaline conditions, so that the surface of the hydrothermal titanate colloidal particles is negatively charged, resulting in electrostatic repulsion, effectively preventing the particles from approaching and aggregating, and improving the dispersion stability; in addition, the π bond of the dopamine side chain can form a coordination bond with the d empty orbital of the metal atom, so that the dopamine side chain is firmly adsorbed on the surface of the titanate particles, and when the amide group in the dopamine side chain is close to the π bond, a larger π bond system is formed due to the conjugation effect, which significantly enhances the adsorption force of the derivative on the metal atom, thereby firmly anchoring the derivative on the surface of the titanate colloidal particles, preventing the loss of the dispersant, and maintaining a stable and lasting dispersion effect; finally, the spatial structure of the polymer main chain and the side chain forms a protective layer on the particle surface, further preventing the particles from aggregating through a steric barrier effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show schematic diagrams of certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0034] Figure 1 This is a SEM photograph of the high-purity titanium dioxide prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0035] In order to make the purpose, technical solution and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with embodiments. Of course, the specific embodiments described here are only used to explain the present invention and are not used to limit the present invention.

[0036] Unless otherwise specified, the chemical reagents and materials in the present invention are purchased from commercial sources or synthesized from raw materials purchased from commercial sources.

[0037] Polysuccinimide with a molecular weight of 5000 was purchased from Shanghai MacLean Biochemical Technology Co., Ltd.

[0038] The titanium-containing blast furnace slag used in the embodiments and comparative examples comes from a domestic factory, and its chemical composition is shown in Table 1:

[0039] Table 1 Main composition of titanium-containing blast furnace slag

[0040]

[0041] A method for preparing high-purity spherical titanium dioxide comprises the following steps:

[0042] (1) dissolving 40 mmol of polysuccinimide in 15 mL of DMSO to obtain a PSI solution; dissolving 10-15 mmol of dopamine hydrochloride in 15 mL of DMSO, then adding 8-16 mL of triethylamine, and ultrasonically oscillating for 10-30 min to obtain a dopamine solution; adding the dopamine solution to the PSI solution, and refluxing for 18-30 h at 50-70° C. in a nitrogen atmosphere to obtain a PSI-DA intermediate reaction solution;

[0043] (2) dissolving 30-25 mmol of glutamic acid in DMSO, then adding 10-20 mL of triethylamine, and ultrasonically oscillating for 10-30 min to obtain a glutamic acid solution; adding the glutamic acid solution to the intermediate reaction solution, stirring and reacting for 12-20 h at 50-70° C. in a nitrogen atmosphere, adjusting the pH to 7-8 with an aqueous sodium hydroxide solution, precipitating the product with acetone, filtering, washing with acetone, and drying to obtain a polysuccinimide derivative;

[0044] (3) crushing and grinding the titanium-containing blast furnace slag and passing it through a 200-600 mesh sieve;

[0045] (4) 1 kg of sieved titanium-containing blast furnace slag is mixed with 1.5-2.2 kg of 85-98 wt% sulfuric acid solution, and 0.1-5 g of citric acid and 5-20 g of sodium dodecylbenzene sulfonate are added, and the mixture is reacted at 70-130° C. for 1-6 h to obtain acid hydrolysis residue; 1 kg of the acid hydrolysis residue is added to 1-2 kg of deionized water, stirred and mixed, and filtered to obtain a solution containing impure sulfuric acid titanium oxide;

[0046] (5) adding 1 kg of the titanium dioxide solution containing heterosulfate and 1 to 30 g of a polysuccinimide derivative into a reaction kettle, and conducting a sealed hydrothermal reaction at 110 to 160° C. and 0.2 to 1 MPa for 1 to 12 h, cooling and filtering the product to obtain a filter cake, and washing and drying the filter cake to obtain hydrothermal metatitanic acid;

[0047] (6) Mixing hydrothermal titanic acid with 0.5-5wt% NaOH solution to form a slurry, adjusting the pH to 10-14, stirring at room temperature at 400-800 r / min for 30-120 min, filtering and washing the product, and drying at 100-110°C for 1-3 h to obtain desulfurized titanic acid; calcining the desulfurized titanic acid in a muffle furnace at 500-1000°C for 2-5 h, and cooling to obtain the high-purity spherical titanium dioxide.

[0048] The present invention will be further described below through specific embodiments.

[0049] Example 1

[0050] A method for preparing high-purity spherical titanium dioxide comprises the following steps:

[0051] (1) Dissolve 40 mmol polysuccinimide in 15 mL DMSO to obtain a PSI solution; dissolve 15 mmol dopamine hydrochloride in 15 mL DMSO, then add 12 mL triethylamine, and ultrasonically oscillate for 30 min to obtain a dopamine solution; add the dopamine solution to the PSI solution, reflux at 60° C. under a nitrogen atmosphere for 26 h to obtain a PSI-DA intermediate reaction solution;

[0052] (2) dissolving 25 mmol of glutamic acid in DMSO, then adding 14 mL of triethylamine, and ultrasonically oscillating for 30 min to obtain a glutamic acid solution; adding the glutamic acid solution to the intermediate reaction solution, stirring and reacting at 60° C. under a nitrogen atmosphere for 16 h, adjusting the pH to 8 with an aqueous sodium hydroxide solution, precipitating the product with acetone, filtering, washing with acetone, and drying to obtain a polysuccinimide derivative;

[0053] (3) crushing and grinding the titanium-containing blast furnace slag and passing it through a 500-mesh sieve;

[0054] (4) 1 kg of sieved titanium-containing blast furnace slag was mixed with 2.2 kg of 95 wt% sulfuric acid solution, and 5 g of citric acid and 20 g of sodium dodecylbenzene sulfonate were added, and the mixture was reacted at 130° C. for 1 h to obtain acid hydrolysis slag; 1 kg of the acid hydrolysis slag was added to 2 kg of deionized water, stirred and mixed, and filtered to obtain a solution containing impure sulfuric acid titanium oxide;

[0055] (5) adding 1 kg of the titanium dioxide solution containing heterosulfate and 15 g of the polysuccinimide derivative into a reaction kettle, and conducting a sealed hydrothermal reaction at 160° C. and 1 MPa for 1 h, cooling and filtering the product to obtain a filter cake, and washing and drying the filter cake to obtain hydrothermal metatitanic acid;

[0056] (6) Mix hydrothermal titanic acid with 5 wt% NaOH solution to form a slurry, adjust the pH to 12, stir at room temperature for 120 min at 600 r / min, filter and wash the product, and dry it at 110°C for 1 h to obtain desulfurized titanic acid; calcine the desulfurized titanic acid in a muffle furnace at 800°C for 3 h, cool it, and obtain anatase-type high-purity spherical titanium dioxide with a purity of 99.87% and a D50 of 54 nm.

[0057] Figure 1 This is a SEM photograph of the high-purity spherical titanium dioxide prepared in Example 1.

[0058] Example 2

[0059] A method for preparing high-purity spherical titanium dioxide comprises the following steps:

[0060] (1) Dissolve 40 mmol polysuccinimide in 15 mL DMSO to obtain a PSI solution; dissolve 13 mmol dopamine hydrochloride in 15 mL DMSO, then add 12 mL triethylamine, and ultrasonically oscillate for 30 min to obtain a dopamine solution; add the dopamine solution to the PSI solution, reflux at 60° C. under a nitrogen atmosphere for 26 h to obtain a PSI-DA intermediate reaction solution;

[0061] (2) dissolving 25 mmol of glutamic acid in DMSO, then adding 14 mL of triethylamine, and ultrasonically oscillating for 30 min to obtain a glutamic acid solution; adding the glutamic acid solution to the intermediate reaction solution, stirring and reacting at 60° C. under a nitrogen atmosphere for 16 h, adjusting the pH to 8 with an aqueous sodium hydroxide solution, precipitating the product with acetone, filtering, washing with acetone, and drying to obtain a polysuccinimide derivative;

[0062] (3) crushing and grinding the titanium-containing blast furnace slag and passing it through a 500-mesh sieve;

[0063] (4) 1 kg of sieved titanium-containing blast furnace slag was mixed with 1.8 kg of 95 wt% sulfuric acid solution, and 2.5 g of citric acid and 12 g of sodium dodecylbenzene sulfonate were added, and the mixture was reacted at 100° C. for 4 h to obtain acid hydrolysis residue; 1 kg of the acid hydrolysis residue was added to 1.5 kg of deionized water, stirred and mixed, and filtered to obtain a solution containing impure sulfuric acid titanium oxide;

[0064] (5) adding 1 kg of the titanium dioxide solution containing heterosulfate and 30 g of the polysuccinimide derivative into a reaction kettle, and conducting a sealed hydrothermal reaction at 140° C. and 0.6 MPa for 66 h, cooling and filtering the product to obtain a filter cake, and washing and drying the filter cake to obtain hydrothermal metatitanic acid;

[0065] (6) Mix hydrothermal titanic acid with 2.5 wt% NaOH solution to form a slurry, adjust the pH to 12, stir at room temperature at 600 r / min for 80 min, filter and wash the product, and dry it at 105°C for 2 h to obtain desulfurized titanic acid; calcine the desulfurized titanic acid in a muffle furnace at 700°C for 4 h, cool it, and obtain anatase-type high-purity spherical titanium dioxide with a purity of 99.95% and a D50 of 63 nm.

[0066] Example 3

[0067] A method for preparing high-purity spherical titanium dioxide comprises the following steps:

[0068] (1) Dissolve 40 mmol polysuccinimide in 15 mL DMSO to obtain a PSI solution; dissolve 10 mmol dopamine hydrochloride in 15 mL DMSO, then add 12 mL triethylamine, and ultrasonically oscillate for 30 min to obtain a dopamine solution; add the dopamine solution to the PSI solution, reflux at 60° C. under a nitrogen atmosphere for 26 h to obtain a PSI-DA intermediate reaction solution;

[0069] (2) 30 mmol of glutamic acid was dissolved in DMSO, and then 14 mL of triethylamine was added, and ultrasonic oscillation was performed for 30 min to obtain a glutamic acid solution; the glutamic acid solution was added to the intermediate reaction solution, and the reaction was stirred at 60° C. under a nitrogen atmosphere for 16 h, and the pH was adjusted to 8 with an aqueous sodium hydroxide solution. The product was precipitated with acetone, filtered, washed with acetone, and dried to obtain a polysuccinimide derivative;

[0070] (3) crushing and grinding the titanium-containing blast furnace slag and passing it through a 500-mesh sieve;

[0071] (4) 1 kg of sieved titanium-containing blast furnace slag was mixed with 1.5 kg of 95 wt% sulfuric acid solution, and 0.1 g of citric acid and 5 g of sodium dodecylbenzene sulfonate were added, and the mixture was reacted at 70° C. for 6 h to obtain acid hydrolysis residue; 1 kg of the acid hydrolysis residue was added to 1 kg of deionized water, stirred and mixed, and filtered to obtain a solution containing impure sulfuric acid titanium oxide;

[0072] (5) adding 1 kg of the titanium dioxide solution containing heterosulfate and 10 g of the polysuccinimide derivative into a reaction kettle, and conducting a sealed hydrothermal reaction at 110° C. and 0.2 MPa for 12 h, cooling and filtering the product to obtain a filter cake, and washing and drying the filter cake to obtain hydrothermal metatitanic acid;

[0073] (6) Mix hydrothermal titanic acid with 0.5 wt% NaOH solution to form a slurry, adjust the pH to 12, stir at room temperature for 30 min at 600 r / min, filter and wash the product, and dry it at 100°C for 3 h to obtain desulfurized titanic acid; calcine the desulfurized titanic acid in a muffle furnace at 900°C for 2 h, cool it, and obtain rutile high-purity spherical titanium dioxide with a purity of 99.92% and a D50 of 47 nm.

[0074] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing high-purity spherical titanium dioxide, characterized in that: The steps include: (1) crushing, grinding and sieving titanium-containing blast furnace slag; (2) mixing the sieved titanium-containing blast furnace slag with a sulfuric acid solution, adding citric acid and sodium dodecylbenzene sulfonate, heating for reaction, and obtaining an acid hydrolysis slag; adding the acid hydrolysis slag into deionized water, stirring and mixing, and filtering to obtain an impure sulfuric acid-containing titanium oxide solution; (3) adding the titanium dioxide solution containing the impurity sulfate and the polysuccinimide derivative into a reaction kettle, sealing the reaction kettle, cooling the product, filtering the product to obtain a filter cake, washing the filter cake, and drying the filter cake to obtain hydrothermal metatitanic acid; (4) mixing hydrothermal metatitanic acid and NaOH solution to form a slurry, adjusting the pH, stirring at room temperature, filtering, washing, and drying the product to obtain desulfurized metatitanic acid; The desulfurized metatitanic acid is roasted and cooled to obtain the high-purity spherical titanium dioxide.

2. The preparation method according to claim 1, characterized in that: In step (1), the product is sieved through a 200-600 mesh sieve.

3. The preparation method according to claim 1, characterized in that: In step (2), the concentration of the sulfuric acid solution is 85-98 wt %; the heating reaction conditions are 70-130° C. for 1-6 hours; the amount ratio of titanium-containing blast furnace slag to sulfuric acid solution is 1:1.5-2.2; The dosage of citric acid and sodium dodecylbenzene sulfonate is 0.01-0.5wt% and 0.5-2wt% of the titanium-containing blast furnace slag respectively; the dosage ratio of the acid-lysed slag and deionized water is 1:1-2.

4. The preparation method according to claim 1, characterized in that: In step (3), the sealed reaction conditions are hydrothermal reaction at 110-160° C. and 0.2-1 MPa for 1-12 hours; the mass ratio of the heterosulfate-containing titanyl solution to the polysuccinimide derivative is 100:0.1-3.

5. The preparation method according to claim 1, characterized in that: In step (4), the concentration of NaOH solution is 0.5-5wt%, and the pH is adjusted to 10-14; the stirring condition at room temperature is stirring at 400-800r / min for 30-120min, the drying condition is drying at 100-110°C for 1-3h; and the calcination condition is calcining in a muffle furnace at 500-1000°C for 2-5h.

6. The preparation method according to claim 1, characterized in that: The preparation method of the polysuccinimide derivative comprises the following steps: a. Dissolve polysuccinimide in DMSO to obtain a PSI solution; dissolve dopamine hydrochloride in DMSO, then add triethylamine, and perform ultrasonic oscillation to obtain a dopamine solution; The dopamine solution was added to the PSI solution, and the mixture was refluxed under a nitrogen atmosphere to obtain a PSI-DA intermediate reaction solution; b. Dissolve glutamic acid in DMSO, then add triethylamine, and perform ultrasonic oscillation to obtain a glutamic acid solution; The glutamic acid solution is added to the intermediate reaction solution, and the reaction is stirred under a nitrogen atmosphere. The pH is adjusted with an aqueous sodium hydroxide solution. The product is precipitated with acetone, filtered, washed with acetone, and dried to obtain the polysuccinimide derivative.

7. The preparation method according to claim 6, characterized in that: In step a, the dosage ratio of PSI, dopamine hydrochloride and triethylamine is 40mmol:10-15mmol:8-16mL; the ultrasonic oscillation time is 10-30min; and the reflux reaction conditions are reflux reaction at 50-70°C for 18-30h.

8. The preparation method according to claim 6, characterized in that: In step b, the ratio of glutamic acid to triethylamine is 30 mmol:10-20 mL; the stirring reaction conditions are 50-70° C. for 12-20 h, and after the reaction, the pH is adjusted to 7-8.

9. The preparation method according to claim 6, characterized in that: The molar ratio of polysuccinimide, dopamine hydrochloride and glutamic acid is 40:10-15:30-25.

10. A high-purity spherical titanium dioxide prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Controllable crystalline form titanium dioxide and graphite alkene composite material with high efficient photoelectricity activity and preparation method thereof

    CN102513079A

  • Method for preparing high-purity titanium dioxide from titanium-containing blast furnace slag

    CN112047377A

  • Method for preparing high-purity nano titanium dioxide by sulfuric acid method and product

    CN115124072A

  • Titanium oxide functional molecule composite particle

    JP2009091345A

Cited By

  • Spherical nano titanium dioxide for lithium ion battery and preparation method of spherical nano titanium dioxide

    CN122212239A