Layered positive electrode precursor of sodium ion battery, preparation method of layered positive electrode precursor, positive electrode material and sodium ion battery
By adopting a layered positive electrode precursor with a specific structure and preparation method in sodium ion batteries, the problem of poor structural stability of the positive electrode material of sodium ion batteries is solved, the cycle stability and energy density are improved, and the efficient energy storage of sodium ion batteries is achieved .
Patent Information
- Application Number
- CN202411079419.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-12
AI Technical Summary
The structural stability of the positive electrode material of sodium ion battery is poor, resulting in insufficient cyclic stability and energy density. Due to the large radius of sodium ions, it affects the structural stability of the material.
The structure formula of the layered positive electrode precursor of sodium ion battery is NiaFebMncMd[(CO3)x(OH)2-2x], and the reaction is carried out in an ammonia solution with pH 8.5-10.8 under the protection of inert gas, and the temperature is controlled by 40-80℃, and the control is carried out. The concentration and feed rate of salt solution and alkali solution ensure uniform precipitation of elements such as nickel, iron, manganese, and improve the structural stability of the transition metal layer.
It effectively improves the structural stability and energy density of the positive electrode material, improves the cycle stability and energy density of sodium ion batteries, avoids segregation and oxidation of metal elements, and ensures uniform distribution and high density of the material.
Smart Images

Figure CN118929787A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of low-cost energy storage batteries, and in particular to a sodium ion battery layered positive electrode precursor and a preparation method thereof, a positive electrode material and a sodium ion battery. Background Art
[0002] The instability of sustainable energy (weather, climate, environmental impact) has led to severe limitations in the practical application of solar energy, tidal energy, wave energy, and wind energy to replace traditional mineral energy represented by coal, oil, and natural gas. Therefore, sustainable, cheap, safe, and environmentally friendly energy storage batteries are needed. In the field of electrochemical energy storage, lithium-ion batteries represented by lithium iron phosphate batteries are currently dominant. However, lithium resources have many development uncertainties due to their resources, prices, and safety. Sodium-ion batteries have similar energy storage mechanisms to lithium-ion batteries, and have the advantages of abundant sodium raw material resources, low cost, and high energy density. Therefore, they have attracted much attention.
[0003] Sodium ion cathode materials are mainly divided into three categories: transition metal layered oxides, polyanion compounds, and Prussian blue compounds. Transition metal layered oxides have developed most rapidly due to their high specific capacity, high working potential, and mature synthesis process. However, the problem of excessively large sodium ion radius means that greater strain will be caused during the ion extraction process, thereby affecting the structural stability of the cathode material. Therefore, there is an urgent need for a sodium ion battery cathode precursor with a stable structure and a preparation method thereof to stabilize the structure of the cathode material. Summary of the invention
[0004] The present invention aims to solve the problem of poor structural stability of positive electrode materials in the prior art and aims to provide a sodium ion battery layered positive electrode precursor and a preparation method thereof, a positive electrode material and a sodium ion battery. The precursor has a good crystal structure and a high tap density, can ensure the structural stability of the positive electrode material, and effectively improve the cycle stability and energy density of the sodium ion battery.
[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0006] A sodium ion battery layered positive electrode precursor, the positive electrode precursor structure is Ni a Fe b Mn c M d [(CO 3 ) x (OH) 2-2x ]; wherein M is one or more of La, Zr, Al, Mg and Ca, a+b+c+d=1, 0.2≤a≤0.5, 0.1≤b≤0.3, 0.2≤c≤0.7, 0≤d≤0.05, 0≤x≤1.
[0007] Furthermore, 0.3≤a≤0.5, 0.2≤b≤0.4, 0.2≤c≤0.5, 0.01≤d≤0.05, 0≤x≤1.
[0008] Furthermore, 0.33≤a≤0.43, 0.3≤b≤0.36, 0.27≤c≤0.33, 0.01≤d≤0.04, 0≤x≤0.8.
[0009] A method for preparing a layered positive electrode precursor for a sodium ion battery comprises the following steps:
[0010] Under the protection of inert gas, a salt solution, an alkaline solution and a second ammonia solution are added to a first ammonia solution at a temperature of 40-80° C., and reacted at a pH of 8.5-10.8 to obtain a layered positive electrode precursor for a sodium ion battery;
[0011] The salt solution is a solution containing one or more of La, Zr, Al, Mg and Ca and Ni, Fe and Mn;
[0012] The cathode precursor structure is Ni a Fe b Mn c M d [(CO 3 ) x (OH) 2-2x ]; wherein M is one or more of La, Zr, Al, Mg and Ca, a+b+c+d=1, 0.2≤a≤0.5, 0.1≤b≤0.3, 0.2≤c≤0.7, 0≤d≤0.05, 0≤x≤1.
[0013] Furthermore, the total concentration of metal ions in the salt solution is 1-2.5 mol / L, the concentration of the first ammonia solution is 0.1-1.2 mol / L, the concentration of the second ammonia solution is 0.8-2 mol / L, and the concentration of the alkaline solution is 2-6 mol / L.
[0014] Further, the alkaline solution is NaOH and / or Na 2 CO 3 Solution.
[0015] Furthermore, after adding the salt solution, the alkaline solution and the second ammonia solution to the first ammonia solution at 40-80° C., the instantaneous feed ammonia concentration is 0.1-1.2 mol / L.
[0016] Furthermore, the instantaneous feed ammonia concentration is calculated by the following formula:
[0017] C=C1*V1 / (V2+V3+V1)
[0018] Wherein, C is the instantaneous ammonia concentration, C1 is the concentration of the second ammonia solution, V1 is the feed rate of the second ammonia solution, V2 is the feed rate of the salt solution, and V3 is the feed rate of the alkaline solution.
[0019] Furthermore, the time from the addition of the salt solution, the alkaline solution and the second ammonia solution to the first ammonia solution at a temperature of 40-80° C. to the completion of the reaction is 30-50 hours.
[0020] Further, the reaction is carried out at a stirring rate of 600-1000 r / min.
[0021] A sodium ion battery layered positive electrode material is prepared by mixing the positive electrode precursor with sodium carbonate and then sintering.
[0022] A sodium ion battery comprises a positive electrode, a negative electrode and an electrolyte, wherein the positive electrode comprises the sodium ion battery layered positive electrode material.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] The present invention continuously introduces inert gas during the preparation process of the layered positive electrode precursor of the sodium ion battery, thereby suppressing the oxidation of divalent iron ions in the reaction system and the raw materials, and effectively suppressing the segregation problem of metal elements.
[0025] Since the layered positive electrode of the sodium ion battery is mainly composed of a transition metal layer and a sodium ion layer, the sodium ion layer not only provides sodium deintercalation sites but also contributes to the support of the material structure, while the transition metal layer provides electrons and supports the material structure. During the charge and discharge process, the structural stability of the transition metal layer determines the stability of the positive electrode material. Therefore, in order to ensure the structural stability of the transition metal layer, it is necessary to ensure the uniform distribution of each element in the transition metal layer. According to the ratio between the elements of the salt solution and the type and content of the doping elements, the present invention controls the pH between 8.5-10.8 and the temperature between 40-80°C, which can ensure the co-precipitation of nickel, iron, manganese and other elements, thereby ensuring the uniformity of the distribution of the precursor elements and the precursor structure, and then ensuring the uniform distribution of the transition metal layer elements of the layered positive electrode, thereby improving the stability of the layered positive electrode structure, increasing the depth of sodium deintercalation of the layered positive electrode, and improving the energy density.
[0026] Furthermore, by increasing the compaction density of the layered positive electrode, the energy density of the material can also be effectively improved. Since there is structural inheritance between the precursor and the layered positive electrode, increasing the compaction density of the precursor can effectively increase the compaction density of the positive electrode material. The present invention prepares a precursor with high density by regulating the raw material concentration, feed rate, and stirring speed, effectively increasing the compaction density of the precursor, and then increasing the compaction density of the positive electrode material.
[0027] Furthermore, by regulating the NaOH and Na 2 CO 3 The ratio between them can effectively control the element distribution, morphology and size of the primary particles of the precursor, and then control the secondary particle precursor formed by the agglomeration of the primary particles, thereby effectively improving the element distribution and compaction density of the precursor.
[0028] Furthermore, according to the preparation requirements of the positive electrode material, the type of transition metal elements can be effectively controlled in the precursor preparation stage. By adjusting the parameters such as the alkaline solution ratio, the system pH, and the instantaneous feed ammonia concentration, the precursor structure is ensured while ensuring the uniform distribution of transition metal elements in the precursor, thereby preparing a positive electrode material with high capacity and stable structure.
[0029] Furthermore, the stirring rate is 600-1000 r / min. The stirring speed should not be too slow, which will cause the size of the precursor particle agglomerates to be too large, which is not conducive to improving the tap density; if it is too high, it will inhibit the agglomeration process and affect the uniformity of the size distribution.
[0030] The precursor of the present invention has a good crystal structure and a high tap density, which can ensure the structural stability of the positive electrode material and effectively improve the cycle stability and energy density of the sodium ion battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a SEM image of the sodium ion battery precursor prepared in Example 1;
[0032] Figure 2 This is a SEM image of the sodium ion battery precursor prepared in Example 2;
[0033] Figure 3 The charge and discharge curve at 0.1C of a sodium ion battery assembled from a layered sodium ion battery positive electrode material prepared using the sodium ion battery precursor prepared in Example 2 as a raw material;
[0034] Figure 4 This is the SEM image of the sodium ion battery precursor prepared in Example 3. DETAILED DESCRIPTION
[0035] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly and comprehensively understood.
[0036] The present invention discloses a sodium ion battery layered positive electrode precursor, the general structural formula of which is Ni a Fe bMn c M d [(CO 3 ) x (OH) 2-2x ]; wherein M is one or more of La, Zr, Al, Mg and Ca, a+b+c+d=1, 0.2≤a≤0.5, 0.1≤b≤0.3, 0.2≤c≤0.7, 0≤d≤0.05, 0≤x≤1.
[0037] The method for preparing a layered positive electrode precursor for a sodium ion battery of the present invention comprises the following steps:
[0038] (1) Prepare a salt solution, an alkaline solution and a second ammonia solution. The salt solution contains Ni, Fe and Mn, and one or more of La, Zr, Al, Mg and Ca are added as required, and the concentration of the salt solution is between 1-2.5 mol / L; the alkaline solution is composed of NaOH and Na 2 CO 3 The solution is prepared by mixing one or two of the above, and the concentration of the solution is between 2-6 mol / L; the concentration of the second ammonia solution is between 0.8-2 mol / L; and an inert gas is charged into the salt solution.
[0039] (2) filling the reaction device with an inert gas and adding a reaction base liquid, wherein the base liquid is a first ammonia solution, and the concentration of the first ammonia solution is between 0.1 and 1.2 mol / L;
[0040] (3) The base liquid is heated to a reaction control temperature (between 40°C and 80°C, for example, 40°C, 50°C, 55°C, 60°C, 70°C or 80°C), and then the salt solution, the alkaline solution and the second ammonia solution are added to the reaction device in parallel, and the pH of the reaction system is simultaneously controlled to be 8.5-10.8 (for example, 8.5, 9.5, 10.0, 10.5 or 10.8, etc.).
[0041] (4) In step (3), the feed rate of the salt solution is 2-6 ml / min, the feed rate of the alkaline solution fluctuates within a certain range according to the pH requirement of the system, and the feed rate of the second ammonia solution maintains the instantaneous ammonia concentration of the overall feed between 0.1 and 1.2 mol / L.
[0042] Instantaneous ammonia concentration C = C1*V1 / (V2+V3+V1)
[0043] Wherein, C is the instantaneous feed ammonia concentration, C1 is the concentration of the second ammonia solution, V1 is the feed rate of the second ammonia solution, V2 is the feed rate of the salt solution, and V3 is the feed rate of the alkaline solution.
[0044] (5) The stirring rate of the reaction device in step (3) is 600-1000 r / min, for example 600 r / min, 650 r / min, 700 r / min or 800 r / min. The stirring speed should not be too slow, otherwise the size of the precursor particle agglomerates will be too large, which is not conducive to improving the tap density; if it is too high, it will inhibit the agglomeration process and affect the uniformity of the size distribution.
[0045] (6) The reaction time of step (3) (i.e., the time from the time when the salt solution, the alkaline solution and the ammonia solution are added to the reaction device in parallel to the time when the reaction is completed) is controlled to be 30-50 hours. The slurry after the reaction is washed with water 4-5 times and then dried at 120° C. for more than 24 hours to finally obtain a layered positive electrode precursor for a sodium ion battery.
[0046] A sodium ion battery layered positive electrode material is prepared by mixing the positive electrode precursor with sodium carbonate and then sintering.
[0047] A sodium ion battery comprises a positive electrode, a negative electrode and an electrolyte, wherein the positive electrode comprises the sodium ion battery layered positive electrode material.
[0048] The following are specific embodiments.
[0049] Example 1
[0050] (1) preparing a nickel, iron, manganese and lanthanum sulfate solution with a total metal ion concentration of 1.5 mol / L, wherein the molar ratio of nickel, iron and manganese in the salt solution is 1:1.1:0.9:0.01; preparing a mixed alkaline solution of sodium carbonate and sodium hydroxide with a concentration of 4 mol / L, wherein the molar ratio of sodium carbonate to sodium hydroxide is 2:1; preparing a second ammonia solution with a concentration of 1.5 mol / L; and then introducing an inert gas into the salt solution.
[0051] (2) adding a base liquid to the reaction device, wherein the base liquid is a first ammonia solution with a concentration of 0.5 mol / L;
[0052] (3) The three prepared solutions are added to the reaction device simultaneously, and an inert gas is introduced into the reaction device at the same time to carry out a coprecipitation reaction. The stirring speed is controlled to be 600r / min, the temperature of the reaction system is 55°C, and the pH of the reaction system is controlled to be 8.5. Among them, the rate of addition of the salt solution is 2ml / min, the rate of addition of the alkaline solution fluctuates within a certain range to keep the pH of the system stable, and the feed rate of the second ammonia solution keeps the instantaneous ammonia concentration of the feed at 0.5mol / L (instantaneous ammonia concentration = second ammonia solution concentration * second ammonia solution feed rate / (salt solution feed rate + alkaline solution feed rate + second ammonia solution feed rate)).
[0053] (4) After the reaction in step (3) is completed for 50 hours, the slurry is washed three times with water, the pH of the supernatant is tested to be between 7 and 7.5, and then dried at 120° C. for 24 hours to finally obtain a layered sodium ion battery precursor.
[0054] The structure of a sodium ion battery layered positive electrode precursor prepared in this embodiment is Ni a Fe b Mn c M d [(CO 3 ) x (OH) 2-2x ]; where M is La, a is 0.33, b is 0.36, c is 0.3, d is 0.01, and x is 0.8.
[0055] The precursor prepared in this example has good sphericity, and the three elements are evenly distributed in the precursor. Figure 1 As shown. By scanning the image and measuring, it can be concluded that the size of the precursor is about 10μm.
[0056] Example 2
[0057] (1) preparing a nickel, iron and manganese sulfate solution with a total metal ion concentration of 2.0 mol / L, wherein the molar ratio of nickel, iron and manganese in the salt solution is 1.3:0.9:0.8; preparing a mixed alkaline solution of sodium carbonate and sodium hydroxide with a concentration of 4 mol / L, wherein the molar ratio of sodium carbonate to sodium hydroxide is 1:3; preparing a second ammonia solution with a concentration of 2 mol / L; and then introducing an inert gas into the salt solution.
[0058] (2) adding a base liquid to the reaction device, wherein the base liquid is a first ammonia solution with a concentration of 0.5 mol / L;
[0059] (3) The three prepared solutions are added to the reaction device simultaneously, and an inert gas is introduced into the reaction device at the same time to carry out a co-precipitation reaction. The stirring speed is controlled to be 800r / min, the temperature of the reaction system is 55°C, and the pH of the reaction system is controlled to be 9.5. Among them, the rate of addition of the salt solution is 2ml / min, the rate of addition of the alkaline solution fluctuates within a certain range to keep the pH of the system stable, and the feed rate of the second ammonia solution keeps the instantaneous ammonia concentration of the feed at 0.5mol / L (instantaneous ammonia concentration = second ammonia solution concentration * second ammonia solution feed rate / (salt solution feed rate + alkaline solution feed rate + second ammonia solution feed rate))
[0060] (4) After the reaction in step (3) is completed for 50 hours, the slurry is washed three times with water, the pH of the supernatant is tested to be between 7 and 7.5, and then dried at 120° C. for 24 hours to finally obtain a layered sodium ion battery precursor.
[0061] The structure of a sodium ion battery layered positive electrode precursor prepared in this embodiment is Ni a Fe b Mn c M d [(CO 3 ) x (OH) 2-2x ]; where a is 0.43, b is 0.3, c is 0.27, and x is 0.04.
[0062] The precursor primary particles prepared in this example have good structure and uniform element distribution. Figure 2 ) It can be seen that the overall sphericity is good and the size distribution is uniform.
[0063] The precursor was used as a raw material and mixed with sodium carbonate and then sintered to prepare a sodium ion battery layered positive electrode. The prepared sodium ion battery layered positive electrode had a specific capacity of up to 151 mAh / g, and the charge and discharge curves were as follows: Figure 3 shown.
[0064] Example 3
[0065] (1) preparing a nickel, iron, manganese, and zirconium sulfate solution with a total metal ion concentration of 2.5 mol / L, wherein the molar ratio of the four elements of nickel, iron, manganese, and zirconium in the salt solution is 1:1:1:0.03; preparing a sodium hydroxide solution with a concentration of 4 mol / L; preparing a second ammonia solution with a concentration of 0.8 mol / L; and then introducing an inert gas into the salt solution.
[0066] (2) adding a base liquid to the reaction device, wherein the base liquid is a first ammonia solution with a concentration of 0.4 mol / L;
[0067] (3) The three prepared solutions are added to the reaction device simultaneously, and an inert gas is introduced into the reaction device at the same time to carry out a co-precipitation reaction. The stirring speed is controlled to be 1000r / min, the temperature of the reaction system is 50°C, and the pH of the reaction system is controlled at 10.5. Among them, the addition rate of the salt solution is 2.8ml / min, the addition rate of the alkaline solution fluctuates within a certain range to keep the pH of the system stable, and the feed rate of the second ammonia solution keeps the instantaneous ammonia concentration of the feed at 0.4mol / L (instantaneous ammonia concentration = second ammonia solution concentration * second ammonia solution feed rate / (salt solution feed rate + alkaline solution feed rate + second ammonia solution feed rate))
[0068] (4) After 50 hours of reaction in step (3), the slurry was washed three times with water, and the pH of the supernatant was tested to be between 7 and 7.5. The slurry was dried at 120° C. for 24 hours to finally obtain a layered sodium ion battery precursor.
[0069] The structure of a sodium ion battery layered positive electrode precursor prepared in this embodiment is Ni a Fe b Mn c M d (OH) 2 ; Wherein, M is Zr, a is 0.33, b is 0.33, c is 0.33, and d is 0.01.
[0070] See also Figure 4 It can be seen that the precursor prepared in this example has a good primary particle structure, excellent secondary particle density, and a tap density of up to 2.05 g / cm 3 .
[0071] Example 4
[0072] (1) preparing a nickel, iron, manganese, and lanthanum sulfate solution with a total metal ion concentration of 1 mol / L, wherein the molar ratio of the four elements of nickel, iron, manganese, and lanthanum in the salt solution is 1:1:1:0.02; preparing a sodium hydroxide solution with a concentration of 6 mol / L; preparing a second ammonia solution with a concentration of 2.0 mol / L; and then introducing an inert gas into the salt solution.
[0073] (2) adding a base liquid to the reaction device, wherein the base liquid is a first ammonia solution with a concentration of 0.1 mol / L;
[0074] (3) The three prepared solutions are added to the reaction device simultaneously, and an inert gas is introduced into the reaction device at the same time to carry out a co-precipitation reaction. The stirring speed is controlled to be 1000r / min, the temperature of the reaction system is 40°C, and the pH of the reaction system is controlled at 8.5. Among them, the rate of adding the salt solution is 2ml / min, the rate of adding the alkaline solution fluctuates within a certain range to keep the pH of the system stable, and the feed rate of the second ammonia solution keeps the instantaneous ammonia concentration of the feed at 0.1mol / L (instantaneous ammonia concentration = second ammonia solution concentration * second ammonia solution feed rate / (salt solution feed rate + alkaline solution feed rate + second ammonia solution feed rate))
[0075] (4) After 40 hours of reaction in step (3), the slurry was washed three times with water, and the pH of the supernatant was tested to be between 7 and 7.5. The slurry was dried at 120° C. for 24 hours to finally obtain a layered sodium ion battery precursor.
[0076] The structure of a sodium ion battery layered positive electrode precursor prepared in this embodiment is Ni a Fe b Mn c M d [(CO 3 ) x (OH) 2-2x]; wherein M is lanthanum, a is 0.33, b is 0.33, c is 0.33, d is 0.01, and x is 0.
[0077] Example 5
[0078] (1) preparing a nickel, iron, manganese, aluminum, and magnesium sulfate solution with a total metal ion concentration of 2.5 mol / L, wherein the molar ratio of the five elements nickel, iron, manganese, aluminum, and magnesium in the salt solution is 1:1:1:0.02:0.02; preparing a sodium hydroxide solution with a concentration of 2 mol / L; preparing a second ammonia solution with a concentration of 2 mol / L; and then introducing an inert gas into the salt solution.
[0079] (2) adding a base liquid to the reaction device, wherein the base liquid is a first ammonia solution with a concentration of 1 mol / L;
[0080] (3) The three prepared solutions are added to the reaction device simultaneously, and an inert gas is introduced into the reaction device at the same time to carry out a co-precipitation reaction. The stirring speed is controlled to be 800r / min, the temperature of the reaction system is 55°C, and the pH of the reaction system is controlled to be 10.8. Among them, the rate of addition of the salt solution is 6ml / min, the rate of addition of the alkaline solution fluctuates within a certain range to keep the pH of the system stable, and the feed rate of the second ammonia solution keeps the instantaneous ammonia concentration of the feed at 1mol / L (instantaneous ammonia concentration = concentration of the second ammonia solution * feed rate of the second ammonia solution / (feed rate of salt solution + feed rate of alkaline solution + feed rate of the second ammonia solution))
[0081] (4) After 30 hours of reaction in step (3), the slurry was washed three times with water, the pH of the supernatant was tested to be between 7 and 7.5, and dried at 120° C. for 24 hours to finally obtain a layered sodium ion battery precursor.
[0082] The structure of a sodium ion battery layered positive electrode precursor prepared in this embodiment is Ni a Fe b Mn c M d [(CO 3 ) x (OH) 2-2x ]; wherein M is aluminum and magnesium, a is 0.33, b is 0.33, c is 0.33, d is 0.01, and x is 0.
[0083] Example 6
[0084] (1) preparing a nickel, iron and manganese sulfate solution with a total metal ion concentration of 1.2 mol / L, wherein the molar ratio of nickel, iron and manganese in the salt solution is 1:1.1:0.9; preparing a sodium carbonate solution with a concentration of 3 mol / L; preparing a second ammonia solution with a concentration of 0.8 mol / L; and then introducing an inert gas into the salt solution.
[0085] (2) adding a base liquid to the reaction device, wherein the base liquid is a first ammonia solution with a concentration of 0.4 mol / L;
[0086] (3) The three prepared solutions are added to the reaction device simultaneously, and an inert gas is introduced into the reaction device at the same time to carry out a co-precipitation reaction. The stirring speed is controlled to be 700r / min, the temperature of the reaction system is 60°C, and the pH of the reaction system is controlled to be 9.5. Among them, the rate of adding the salt solution is 3ml / min, the rate of adding the alkaline solution fluctuates within a certain range to keep the pH of the system stable, and the feed rate of the second ammonia solution keeps the instantaneous ammonia concentration of the feed at 0.3mol / L (instantaneous ammonia concentration = concentration of the second ammonia solution * feed rate of the second ammonia solution / (feed rate of salt solution + feed rate of alkaline solution + feed rate of the second ammonia solution))
[0087] (4) After the reaction in step (3) for 35 hours is completed, the slurry is washed three times with water, the pH of the supernatant is tested to be between 7 and 7.5, and then dried at 120° C. for 24 hours to finally obtain a layered sodium ion battery precursor.
[0088] Example 7
[0089] (1) preparing a nickel, iron and manganese sulfate solution with a total metal ion concentration of 2.3 mol / L, wherein the molar ratio of nickel, iron and manganese in the salt solution is 1:1.1:0.9; preparing a sodium hydroxide solution with a concentration of 5 mol / L; preparing a second ammonia solution with a concentration of 1.5 mol / L; and then introducing an inert gas into the salt solution.
[0090] (2) adding a base liquid to the reaction device, wherein the base liquid is a first ammonia solution with a concentration of 0.8 mol / L;
[0091] (3) The three prepared solutions are added to the reaction device simultaneously, and an inert gas is introduced into the reaction device at the same time to carry out a coprecipitation reaction. The stirring speed is controlled to be 650r / min, the temperature of the reaction system is 70°C, and the pH of the reaction system is controlled at 10. Among them, the addition rate of the salt solution is 4ml / min, the addition rate of the alkaline solution fluctuates within a certain range to keep the pH of the system stable, and the feed rate of the second ammonia solution keeps the instantaneous ammonia concentration of the feed at 0.8mol / L (instantaneous ammonia concentration = second ammonia solution concentration * second ammonia solution feed rate / (salt solution feed rate + alkaline solution feed rate + second ammonia solution feed rate))
[0092] (4) After the reaction in step (3) is completed for 50 hours, the slurry is washed three times with water, the pH of the supernatant is tested to be between 7 and 7.5, and then dried at 120° C. for 24 hours to finally obtain a layered sodium ion battery precursor.
[0093] Example 8
[0094] (1) preparing a nickel, iron and manganese sulfate solution with a total metal ion concentration of 2 mol / L, wherein the molar ratio of nickel, iron and manganese in the salt solution is 1:1.1:0.9; preparing a sodium hydroxide solution with a concentration of 4 mol / L; preparing a second ammonia solution with a concentration of 2 mol / L; and then introducing an inert gas into the salt solution.
[0095] (2) adding a base liquid to the reaction device, wherein the base liquid is a first ammonia solution with a concentration of 1 mol / L;
[0096] (3) The three prepared solutions are added to the reaction device simultaneously, and an inert gas is introduced into the reaction device at the same time to carry out a co-precipitation reaction. The stirring speed is controlled to be 600r / min, the temperature of the reaction system is 80°C, and the pH of the reaction system is controlled at 10.5. Among them, the rate of addition of the salt solution is 5ml / min, the rate of addition of the alkaline solution fluctuates within a certain range to keep the pH of the system stable, and the feed rate of the second ammonia solution keeps the instantaneous ammonia concentration of the feed at 0.6mol / L (instantaneous ammonia concentration = second ammonia solution concentration * second ammonia solution feed rate / (salt solution feed rate + alkaline solution feed rate + second ammonia solution feed rate))
[0097] (4) After the reaction in step (3) is completed for 50 hours, the slurry is washed three times with water, the pH of the supernatant is tested to be between 7 and 7.5, and then dried at 120° C. for 24 hours to finally obtain a layered sodium ion battery precursor.
[0098] Correspondingly, the positive electrode material prepared by sintering the positive electrode precursor and sodium carbonate also has a better compaction density (≥3.2g / cm 3 ) and specific capacity (≥145mAh / g).
[0099] The above description is only for the best embodiment of the present invention, but it should not be understood as limiting the claims. The present invention is not limited to the above embodiments, and its specific structure is allowed to be changed. However, all changes made within the protection scope of the independent claims of the present invention are within the protection scope of the present invention.
[0100] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
Claims
1. A sodium ion battery layered positive electrode precursor, characterized in that: The positive electrode precursor structural formula is Ni a Fe b Mn c M d [(CO3) x (OH) 2-2x ]; wherein M is one or more of La, Zr, Al, Mg and Ca, a+b+c+d=1, 0.2≤a≤0.5, 0.1≤b≤0.3, 0.2≤c≤0.7, 0≤d≤0.05, 0≤x≤1.
2. A method for preparing a layered positive electrode precursor for a sodium ion battery, characterized in that: The following steps are involved: Under the protection of inert gas, a salt solution, an alkaline solution and a second ammonia solution are added to a first ammonia solution at a temperature of 40-80° C., and reacted at a pH of 8.5-10.8 to obtain a layered positive electrode precursor for a sodium ion battery; The salt solution is a solution containing one or more of La, Zr, Al, Mg and Ca and Ni, Fe and Mn; The cathode precursor structure is Ni a Fe b Mn c M d [(CO3) x (OH) 2-2x ]; wherein M is one or more of La, Zr, Al, Mg and Ca, a+b+c+d=1, 0.2≤a≤0.5, 0.1≤b≤0.3, 0.2≤c≤0.7, 0≤d≤0.05, 0≤x≤1.
3. The method for preparing a layered positive electrode precursor for a sodium ion battery according to claim 2, characterized in that: The total concentration of metal ions in the salt solution is 1-2.5 mol / L, the concentration of the first ammonia solution is 0.1-1.2 mol / L, the concentration of the second ammonia solution is 0.8-2 mol / L, and the concentration of the alkaline solution is 2-6 mol / L.
4. The method for preparing a layered positive electrode precursor for a sodium ion battery according to claim 2, characterized in that: The alkaline solution is NaOH and / or Na2CO3 solution.
5. The method for preparing a layered positive electrode precursor for a sodium ion battery according to claim 2, characterized in that: After adding the salt solution, the alkaline solution and the second ammonia solution to the first ammonia solution at a temperature of 40-80° C., the instantaneous feed ammonia concentration is 0.1-1.2 mol / L.
6. The method for preparing a layered positive electrode precursor for a sodium ion battery according to claim 5, characterized in that: The instantaneous feed ammonia concentration is calculated by the following formula: C=C1*V1 / (V2+V3+V1) Wherein, C is the instantaneous ammonia concentration, C1 is the concentration of the second ammonia solution, V1 is the feed rate of the second ammonia solution, V2 is the feed rate of the salt solution, and V3 is the feed rate of the alkaline solution.
7. The method for preparing a layered positive electrode precursor for a sodium ion battery according to claim 2, characterized in that: The time from adding the salt solution, the alkaline solution and the second ammonia solution to the first ammonia solution at a temperature of 40-80° C. to the end of the reaction is 30-50 hours.
8. The method for preparing a layered positive electrode precursor for a sodium ion battery according to claim 2, characterized in that: The reaction was carried out at a stirring rate of 600-1000 r / min.
9. A layered positive electrode material for a sodium ion battery, characterized in that: The positive electrode precursor according to claim 1 is mixed with sodium carbonate and then sintered.
10. A sodium ion battery comprising a positive electrode, a negative electrode and an electrolyte, characterized in that: The positive electrode comprises the sodium ion battery layered positive electrode material according to claim 9.
Citation Information
Cited By
Precursor of sodium ion battery positive electrode material and preparation method and application thereof
CN121894713A