High-wear-resistance microfiber leather and preparation method thereof

The microfiber is solved by adopting a multi-layer structural design in the microfiber leather, including the base layer, fiber layer, resin layer, wear-resistant layer and backing layer, and adding materials such as alumina and silicon carbide to the wear-resistant layer. The problem of wear and bleaching in extreme conditions significantly improves wear resistance and service life.

CN118932734APending Publication Date: 2024-11-12TIANSHOU FUJIAN SUPERFIBER TECH
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411098826.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing microfiber leather is prone to wear and bleaching under long-term high-strength use and extreme conditions (such as outdoor exposure to the sun and frequent friction), which affects its durability.

Method used

Adopt a multi-layer structural design, including a substrate layer, fiber layer, resin layer, wear-resistant layer and backing layer. By adding materials such as alumina and silicon carbide to the wear-resistant layer, hardness and wear resistance are enhanced, and the hardness and wear resistance are enhanced. Anti-aging agent is added to the grinding layer to absorb UV light and trap free radicals to prevent material from aging.

Benefits of technology

It significantly improves the wear resistance and service life of the ultra-fiber leather under extreme use conditions, and extends the service life of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932734A_ABST
    Figure CN118932734A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of microfiber leather, and discloses high-wear-resistance microfiber leather and a preparation method thereof.The high-wear-resistance microfiber leather comprises a base material layer, a fiber layer, a resin layer, a wear-resistant layer and a backing layer. According to the high-wear-resistance microfiber leather, the hardness and the wear resistance of the microfiber leather can be improved by adding aluminum oxide into the wear-resistant layer, and the wear resistance and the scratch resistance of the coating can be further improved by adding silicon carbide as a reinforcing filler, so that the wear resistance and the scratch resistance of the microfiber leather are improved; meanwhile, the anti-aging agent is added into the wear-resistant layer and can absorb ultraviolet rays and convert the ultraviolet rays into harmless heat energy, so that the microfiber leather is prevented from being damaged by the ultraviolet rays, meanwhile, free radicals generated by ultraviolet irradiation can be captured and quenched, the free radical chain reaction is interrupted, material aging is prevented, and the service life of the product is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ultra-fine leather, and in particular to a highly wear-resistant ultra-fine leather and a preparation method thereof. Background Art

[0002] Superfine fiber synthetic leather is referred to as superfine leather. It is based on sea island fiber nonwoven fabric, impregnated with polyurethane slurry and wet coagulated to form sea island fiber / polyurethane composite material, and then through fiber opening (dissolution method, alkali reduction or toluene reduction), a superfine fiber / polyurethane composite material, that is, superfine fiber synthetic leather base cloth, is obtained. Finally, after different finishing processes, it can produce smooth superfine leather or suede superfine leather with wear resistance, cold resistance, breathability and aging resistance. It has become an ideal material to replace natural leather. Compared with the wet synthetic leather process, the biggest difference between the superfine leather process and the wet synthetic leather process is that the fiber is opened after impregnation and coagulation to turn the sea island fiber into superfine fiber. Because the fiber of superfine leather is very fine, it is closer to natural leather in terms of microstructure and performance, and has better mechanical properties.

[0003] Although the current microfiber leather has good wear resistance, it may still be subject to wear and tear and pilling under long-term and high-intensity use. Especially under extreme usage conditions, such as long-term outdoor exposure and frequent friction, its durability may be affected to a certain extent. Summary of the invention

[0004] In view of the fact that the above-mentioned existing products may still suffer from wear and fuzzing under long-term and high-intensity use, especially under extreme use conditions, such as long-term outdoor exposure and frequent friction, their durability may be affected to a certain extent, the present invention is proposed.

[0005] Therefore, the purpose of the present invention is to provide a highly wear-resistant microfiber leather, the purpose of which is to improve the wear resistance of the microfiber leather under extreme use conditions, such as long-term outdoor exposure and frequent friction.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions: a highly wear-resistant microfiber leather, comprising a substrate layer, a fiber layer, a resin layer, a wear-resistant layer and a backing layer; the fiber layer is bonded to one side of the substrate layer, the backing layer is bonded to the other side of the substrate layer, the resin layer is bonded to the side of the fiber layer away from the substrate layer, and the wear-resistant layer is bonded to the side of the resin layer away from the fiber layer, and the thickness of the bonding layer between the wear-resistant layer and the backing layer is 1.5 mm.

[0007] As a preferred solution of the highly wear-resistant microfiber leather of the present invention, the substrate layer provides basic support and stability, and provides an attachment surface for subsequent layers.

[0008] As a preferred solution of the highly wear-resistant microfiber leather of the present invention, the fiber layer is a three-dimensional structure network made of nylon microfibers through carding, needle punching and other processes.

[0009] As a preferred solution of the highly wear-resistant microfiber leather of the present invention, the resin layer is composed of the following raw materials in parts by weight: 60-75 parts of polyurethane resin, 30-60 parts of diluent and 5-10 parts of color paste.

[0010] As a preferred solution of the highly wear-resistant microfiber leather of the present invention, the diluent is composed of dimethylformamide and methyl ethyl ketone.

[0011] As a preferred embodiment of the highly wear-resistant microfiber leather described in the present invention, the wear-resistant layer is composed of the following raw materials in parts by weight: 100-120 parts of polyurethane resin, 10-20 parts of aluminum oxide, 15-25 parts of silicon carbide, 30-50 parts of anti-aging agent, 5-15 parts of leveling agent, and 8-22 parts of defoaming agent.

[0012] As a preferred solution of the highly wear-resistant microfiber leather of the present invention, the backing layer is composed of the following raw materials in parts by weight: 60-80 parts of polyester fiber and 20-40 parts of PU foam.

[0013] To achieve the above object, the present invention provides the following technical solution: a method for preparing highly wear-resistant microfiber leather, comprising the following steps:

[0014] S1, firstly, a layer of adhesive is coated on one side of the surface of the substrate layer, and then the fiber layer is adhered to one side of the substrate layer, and then sent into an oven for drying;

[0015] S2, preparing a resin layer coating, first taking out an appropriate amount of polyurethane resin and adding an appropriate amount of dimethylformamide and methyl ethyl ketone, putting the mixture into a stirring device and stirring until the polyurethane resin is completely dissolved to form a uniform resin solution, taking out an appropriate amount of color paste according to the desired color, slowly adding the color paste into the resin solution, and stirring the mixture sufficiently to ensure that the color paste is uniformly dispersed in the resin solution, then using a viscometer to detect the viscosity of the coating, adjusting the amount of dimethylformamide and methyl ethyl ketone as needed to achieve a desired viscosity range, and forming a coating;

[0016] S3, coating the coating prepared in S2 on one side of the fiber layer by a coating roller, and then sending the coating into an oven for drying so that a resin layer is attached to the surface of one side of the fiber layer;

[0017] S4, making a wear-resistant coating, first taking out an appropriate amount of polyurethane resin and adding an appropriate amount of aluminum oxide converted into aluminum oxide powder by physical or chemical methods, then adding silicon powder and carbon powder to react at high temperature to generate silicon carbide powder, and then stirring until the polyurethane resin is completely dissolved to form a uniform resin solution, and then adding an appropriate amount of anti-aging agent, leveling agent and defoaming agent and then mixing. After the mixing is completed, the mixed coating is filtered with a filter to remove impurities and particles therein. The filtered coating should be clear and transparent without precipitation and suspended matter. The filtered coating is left to stand for a period of time at an appropriate temperature for maturation. During the maturation process, the components in the coating will fully react and fuse to form a stable coating system;

[0018] S5, coating the coating prepared in S4 on one side of the resin layer by a coating roller, and then sending it into an oven for drying so that a wear-resistant layer is attached to the surface of one side of the resin layer;

[0019] S6, prepare the backing layer coating, add appropriate amount of polyester fiber and PU foam and stir until the polyester fiber is completely dissolved to form a uniform resin solution, then apply the prepared solution on the other side of the substrate layer surface through a coating roller, and then send it into an oven for drying to form a backing layer on one side of the substrate layer.

[0020] The beneficial effects of the present invention are as follows: by adding alumina to the wear-resistant layer, the hardness and wear resistance of the microfiber leather can be improved, and the added silicon carbide can also serve as a reinforcing filler, which can further improve the wear resistance and scratch resistance of the coating, thereby improving the wear resistance and scratch resistance of the microfiber leather. At the same time, an anti-aging agent is added to the wear-resistant layer to absorb ultraviolet rays and convert them into harmless heat energy, thereby preventing ultraviolet rays from damaging the microfiber leather. At the same time, it can capture and quench free radicals generated by ultraviolet radiation, thereby interrupting the free radical chain reaction, preventing material aging, and thus extending the service life of the product. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:

[0022] Figure 1 It is a schematic diagram of the overall structure of the highly wear-resistant microfiber leather of the present invention.

[0023] Description of reference numerals:

[0024] 1. Base material layer; 2. Fiber layer; 3. Resin layer; 4. Wear-resistant layer; 5. Backing layer. DETAILED DESCRIPTION

[0025] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the accompanying drawings.

[0026] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0027] Example 1

[0028] Reference Figure 1 , which is the first embodiment of the present invention, provides a high wear-resistant microfiber leather, the high wear-resistant microfiber leather comprising a substrate layer 1, a fiber layer 2, a resin layer 3, a wear-resistant layer 4 and a backing layer 5;

[0029] The fiber layer 2 is bonded to one side of the substrate layer 1, the backing layer 5 is bonded to the other side of the substrate layer 1, the resin layer 3 is bonded to the side of the fiber layer 2 away from the substrate layer 1, and the wear-resistant layer 4 is bonded to the side of the resin layer 3 away from the fiber layer 2, and the thickness of the bonding layer between the wear-resistant layer 4 and the backing layer 5 is 1.5 mm.

[0030] The substrate layer 1 provides basic support and stability, and provides an attachment surface for subsequent layers. The fiber layer 2 is a three-dimensional structural network made of nylon ultrafine fibers through combing, needle punching and other processes. The diluent is composed of dimethylformamide and methyl ethyl ketone. The diluent is used to adjust the viscosity of the polyurethane resin to make it easier to coat and process.

[0031] The resin layer 3 is composed of the following raw materials in parts by weight: 60 parts of polyurethane resin, 30 parts of diluent and 5 parts of color paste. The polyurethane resin is used as the main elastomeric material to provide tensile properties. In order to give the microfiber leather different colors and appearances, an appropriate amount of color paste needs to be added to the resin layer 3 for color adjustment.

[0032] The wear-resistant layer 4 is composed of the following raw materials in parts by weight: 100 parts of polyurethane resin, 10 parts of aluminum oxide, 15 parts of silicon carbide, 30 parts of anti-aging agent, 5 parts of leveling agent, and 8 parts of defoaming agent. The anti-aging agent can absorb ultraviolet rays and convert them into harmless heat energy, thereby preventing ultraviolet rays from damaging the microfiber leather. At the same time, it can capture and quench free radicals generated by ultraviolet radiation, thereby interrupting the free radical chain reaction and preventing material aging. Aluminum oxide, as a filler, can improve the hardness and wear resistance of the coating. Silicon carbide, also as a reinforcing filler, can further enhance the wear resistance and scratch resistance of the coating. The defoaming agent is used to eliminate bubbles in the preparation and construction process of the coating. The leveling agent is used to improve the leveling and glossiness of the coating.

[0033] The backing layer 5 is composed of the following raw materials in parts by weight: 60 parts of polyester fiber and 20 parts of PU foam. The polyester fiber is used as the main bonding material to firmly bond the backing layer 5 to the substrate layer 1 .

[0034] A method for preparing highly wear-resistant microfiber leather comprises the following steps:

[0035] S1, firstly, a layer of adhesive is applied on one side of the surface of the substrate layer 1, and then the fiber layer 2 is adhered to one side of the substrate layer 1, and then sent into an oven for drying;

[0036] S2, preparing the resin layer 3 coating, firstly taking out a proper amount of polyurethane resin and adding a proper amount of dimethylformamide and methyl ethyl ketone, putting them into a stirring device for stirring, until the polyurethane resin is completely dissolved to form a uniform resin solution, taking out a proper amount of color paste according to the required color, slowly adding the color paste into the resin solution, and stirring sufficiently to ensure that the color paste is evenly dispersed in the resin solution, then using a viscometer to detect the viscosity of the coating, adjusting the amount of dimethylformamide and methyl ethyl ketone as needed to reach the required viscosity range, and forming the coating;

[0037] S3, coating the coating prepared in S2 on one side of the fiber layer 2 by a coating roller, and then sending it into an oven for drying so that a layer of resin layer 3 is attached to the surface of one side of the fiber layer 2;

[0038] S4, making a wear-resistant layer 4 coating, first taking out an appropriate amount of polyurethane resin and adding an appropriate amount of aluminum oxide converted into aluminum oxide powder by physical or chemical methods, then adding silicon powder and carbon powder to react at high temperature to generate silicon carbide powder, and then stirring until the polyurethane resin is completely dissolved to form a uniform resin solution, and then adding an appropriate amount of anti-aging agent, leveling agent and defoaming agent and then mixing. After the mixing is completed, the mixed coating is filtered with a filter to remove impurities and particles therein. The filtered coating should be clear and transparent without precipitation and suspended matter. The filtered coating is left to stand for a period of time at an appropriate temperature for maturation. During the maturation process, the components in the coating will fully react and fuse to form a stable coating system;

[0039] S5, coating the coating prepared in S4 on one side of the resin layer 3 by a coating roller, and then sending it into an oven for drying so that a wear-resistant layer 4 is attached to the surface of one side of the resin layer 3;

[0040] S6, prepare the coating for the backing layer 5, add appropriate amounts of polyester fiber and PU foam and stir until the polyester fiber is completely dissolved to form a uniform resin solution, then apply the prepared solution on the other side of the surface of the substrate layer 1 through a coating roller, and then send it into an oven for drying to form a backing layer 5 on one side of the substrate layer 1.

[0041] Example 2

[0042] Reference Figure 1 , which is the second embodiment of the present invention. This embodiment is different from the first embodiment in that the resin layer 3 is composed of the following raw materials in parts by weight: 68 parts of polyurethane resin, 40 parts of diluent and 7 parts of color paste.

[0043] The wear-resistant layer 4 is composed of the following raw materials in parts by weight: 110 parts of polyurethane resin, 15 parts of aluminum oxide, 20 parts of silicon carbide, 40 parts of anti-aging agent, 8 parts of leveling agent, and 15 parts of defoaming agent.

[0044] The backing layer 5 is composed of the following raw materials in parts by weight: 70 parts of polyester fiber and 30 parts of PU foam.

[0045] The remaining structures are the same as those of Example 1.

[0046] Example 3

[0047] Reference Figure 1 , which is the third embodiment of the present invention. This embodiment is different from the second embodiment in that the resin layer 3 is composed of the following raw materials in parts by weight: 75 parts of polyurethane resin, 60 parts of diluent and 10 parts of color paste.

[0048] The wear-resistant layer 4 is composed of the following raw materials in parts by weight: 120 parts of polyurethane resin, 20 parts of aluminum oxide, 25 parts of silicon carbide, 50 parts of anti-aging agent, 15 parts of leveling agent, and 22 parts of defoaming agent.

[0049] The backing layer 5 is composed of the following raw materials in parts by weight: 80 parts of polyester fiber and 40 parts of PU foam.

[0050] The remaining structure is the same as that of Example 2.

[0051] Microfiber leather abrasion resistance test: According to GB / T3920-2008 "Textile Color Fastness Test-Color Fastness to Friction", the test was conducted using the HT-1004 Martindale Abrasion Tester. The effective diameter of the sample was 2.8 cm. The test results are shown in the following table:

[0052]

[0053] It can be seen from the above table that the microfiber leather prepared by the microfiber leather preparation method used in the present application has excellent wear resistance and scratch resistance.

[0054] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.

Claims

1. A highly wear-resistant microfiber leather, characterized in that: It comprises a substrate layer (1), a fiber layer (2), a resin layer (3), a wear-resistant layer (4) and a backing layer (5); The fiber layer (2) is bonded to one side of the substrate layer (1), the backing layer (5) is bonded to the other side of the substrate layer (1), the resin layer (3) is bonded to the side of the fiber layer (2) away from the substrate layer (1), and the wear-resistant layer (4) is bonded to the side of the resin layer (3) away from the fiber layer (2), and the thickness of the bonding layer between the wear-resistant layer (4) and the backing layer (5) is 1.5 mm.

2. The highly wear-resistant microfiber leather according to claim 1, characterized in that: The substrate layer (1) provides basic support and stability, and provides an attachment surface for subsequent layers.

3. The highly wear-resistant microfiber leather according to claim 2, characterized in that: The fiber layer (2) is a three-dimensional structure network made of nylon ultrafine fibers through processes such as combing and needle punching.

4. The highly wear-resistant microfiber leather according to claim 3, characterized in that: The resin layer (3) is composed of the following raw materials in parts by weight: 60-75 parts of polyurethane resin, 30-60 parts of diluent and 5-10 parts of color paste.

5. The highly wear-resistant microfiber leather according to claim 4, characterized in that: The diluent consists of dimethylformamide and methyl ethyl ketone.

6. The highly wear-resistant microfiber leather according to claim 5, characterized in that: The wear-resistant layer (4) is composed of the following raw materials in parts by weight: 100-120 parts of polyurethane resin, 10-20 parts of aluminum oxide, 15-25 parts of silicon carbide, 30-50 parts of anti-aging agent, 5-15 parts of leveling agent, and 8-22 parts of defoaming agent.

7. The highly wear-resistant microfiber leather according to claim 6, characterized in that: The backing layer (5) is composed of the following raw materials in parts by weight: 60-80 parts of polyester fiber and 20-40 parts of PU foam.

8. A method for preparing a highly wear-resistant microfiber leather, which is applied to the highly wear-resistant microfiber leather described in claim 7, characterized in that: The following steps are included: S1, firstly, a layer of adhesive is coated on one side of the surface of the substrate layer (1), then the fiber layer (2) is adhered to one side of the substrate layer (1), and then the fiber layer (2) is placed in an oven for drying; S2, preparing a resin layer (3) coating, firstly taking out a proper amount of polyurethane resin and adding a proper amount of dimethylformamide and methyl ethyl ketone, putting the mixture into a stirring device and stirring the mixture until the polyurethane resin is completely dissolved to form a uniform resin solution, taking out a proper amount of color paste according to the desired color, slowly adding the color paste into the resin solution, and stirring the mixture sufficiently to ensure that the color paste is uniformly dispersed in the resin solution, then using a viscometer to detect the viscosity of the coating, adjusting the amount of dimethylformamide and methyl ethyl ketone as required to achieve a desired viscosity range, and forming a coating; S3, coating the coating prepared in S2 on one side of the fiber layer (2) by means of a coating roller, and then sending the coating into an oven for drying so that a resin layer (3) is attached to the surface of one side of the fiber layer (2); S4, preparing the wear-resistant layer (4) coating, first taking out an appropriate amount of polyurethane resin and adding an appropriate amount of aluminum oxide converted into aluminum oxide powder by physical or chemical methods, then adding silicon powder and carbon powder to react at high temperature to generate silicon carbide powder, and then stirring until the polyurethane resin is completely dissolved to form a uniform resin solution, and then adding an appropriate amount of anti-aging agent, leveling agent and defoaming agent and then mixing. After mixing, use a filter to filter the mixed coating to remove impurities and particles therein. The filtered coating should be clear and transparent without precipitation and suspended matter. The filtered coating is left to stand for a period of time at an appropriate temperature for maturation. During the maturation process, the components in the coating will fully react and fuse to form a stable coating system; S5, coating the coating prepared in S4 on one side of the resin layer (3) by means of a coating roller, and then sending the coating into an oven for drying so that a wear-resistant layer (4) is attached to the surface of one side of the resin layer (3); S6, preparing a backing layer (5) coating, adding appropriate amounts of polyester fiber and PU foam and stirring until the polyester fiber is completely dissolved to form a uniform resin solution, then coating the prepared solution on the other side of the substrate layer (1) surface through a coating roller, and then sending it into an oven for drying, thereby forming a backing layer (5) on one side of the substrate layer (1).

Citation Information

Cited By

  • Microfiber leather coater and waterproof breathable high-wear-resistance microfiber leather

    CN119838822A

  • A superfine fiber leather coater and a waterproof, breathable and highly wear-resistant superfine fiber leather

    CN119838822B