Gallium oxide piezoelectric substrate and preparation method thereof

By growing crystalline layers on the source substrate and preparing ε-Ga2O3 piezoelectric thin film layer, combined with substrate transfer technology and annealing treatment, the thickness uniformity and crystal phase consistency of the gallium oxide piezoelectric substrate are solved, achieving high Massive gallium oxide piezoelectric substrate preparation improves frequency selectivity of SAW resonators and reduces insertion loss.

CN118944625APending Publication Date: 2024-11-12FUJIAN SUNWISE SEMICON TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410890022.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-06-21
Filing Date
2024-07-04
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing piezoelectric thin film materials such as LiNbO3 and LiTaO3 have poor thickness uniformity, inconsistent crystal phase and high production costs during the preparation process, making it difficult to meet the needs of high-quality and high-precision gallium oxide piezoelectric substrates.

Method used

Grow a crystalline layer on the source substrate, and prepare an ε-Ga2O3 piezoelectric thin film layer on it. The substrate transfer technology is bonded to the transfer substrate and combined with annealing treatment to prepare a gallium oxide pressure with uniform thickness and consistent crystalline phase. The electrical substrate reduces damage to the film layer by removing the substrate.

Benefits of technology

The high-quality requirements of small-size piezoelectric substrates are achieved, the thickness accuracy and uniformity of the ε-Ga2O3 piezoelectric film layer is improved, the insertion loss is reduced, and the frequency selectivity of the SAW resonator is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118944625A_ABST
    Figure CN118944625A_ABST
Patent Text Reader

Abstract

The invention discloses a gallium oxide piezoelectric substrate and a preparation method thereof, and the preparation method comprises the following steps: (1) providing a source substrate, and preparing a crystal layer on the source substrate; (2) preparing an epsilon-Ga2O3 piezoelectric film layer on the crystal layer; (3) preparing a bonding layer on the epsilon-Ga2O3 piezoelectric film layer; (4) providing a transfer substrate, and bonding the epsilon-Ga2O3 piezoelectric film layer with the transfer substrate through a bonding layer; (5) carrying out mechanical thinning and etching on the source substrate to expose the crystal layer; and (6) removing the crystal layer, and exposing the epsilon-Ga2O3 piezoelectric film layer to obtain the gallium oxide piezoelectric substrate. According to the method, the piezoelectric substrate with the high-precision gallium oxide piezoelectric film layer can be prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor technology, and in particular to a gallium oxide piezoelectric substrate and a preparation method thereof. Background Art

[0002] One of the core components of SAW (Surface Acoustic Wave) devices is piezoelectric thin film materials, and the selection of piezoelectric thin film materials has an important impact on the performance of the device. Existing piezoelectric thin film materials usually use ferroelectric single crystal materials such as LiNbO3 and LiTaO3, but the optical devices prepared based on these materials have the disadvantages of poor thickness uniformity of the piezoelectric thin film layer, large device size, low integration, and high production cost. Gallium oxide has the advantages of wide bandgap and high breakdown electric field. Among them, ε-Ga2O3 has a strong piezoelectric polarization effect and can be used as a piezoelectric thin film material. However, epitaxial growth of ε-Ga2O3 on a heterogeneous substrate has the disadvantages of poor thickness uniformity and inconsistent crystal phase. Summary of the invention

[0003] The technical problem to be solved by the present invention is to provide a method for preparing a gallium oxide piezoelectric substrate, which can produce a gallium oxide thin film piezoelectric substrate with high quality and high precision.

[0004] The technical problem to be solved by the present invention is also to provide a gallium oxide piezoelectric substrate with high substrate quality and good acoustic loss suppression effect.

[0005] In order to solve the above technical problems, the present invention provides a method for preparing a gallium oxide piezoelectric substrate, comprising the following steps:

[0006] (1) providing a source substrate and preparing a crystalline layer on the source substrate;

[0007] (2) preparing an ε-Ga2O3 piezoelectric thin film layer on the crystalline layer;

[0008] (3) preparing a bonding layer on the ε-Ga2O3 piezoelectric film layer;

[0009] (4) providing a transfer substrate, and bonding the ε-Ga2O3 piezoelectric thin film layer to the transfer substrate via a bonding layer;

[0010] (5) thinning and etching the source substrate to expose the crystalline layer;

[0011] (6) The crystalline layer is removed to expose the ε-Ga2O3 piezoelectric film layer, thereby obtaining a gallium oxide piezoelectric substrate.

[0012] As an improvement of the above solution, the material of the crystal layer is aluminum nitride and / or silicon carbide, and the thickness is 5nm to 100nm.

[0013] As an improvement of the above solution, the thickness of the ε-Ga2O3 piezoelectric film layer is 100nm to 1000nm.

[0014] As an improvement of the above solution, the ε-Ga2O3 piezoelectric thin film layer is prepared by metal organic chemical vapor deposition, and the growth temperature is 400°C to 600°C.

[0015] As an improvement of the above solution, the material of the bonding layer is one or more of silicon dioxide, silicon nitride, silicon oxynitride, and silicon carbide, and the thickness is 1 μm to 10 μm.

[0016] As an improvement of the above solution, the material of the substrate is one or more of silicon carbide, sapphire, glass, and silicon;

[0017] The material of the transfer substrate is one or more of silicon carbide, sapphire, glass, and silicon.

[0018] As an improvement of the above scheme, step (5) includes the following steps:

[0019] (5.1) Mechanically thinning the source substrate, wherein the thickness of the source substrate after mechanical thinning is 10 μm to 100 μm;

[0020] (5.2) Partially etching the mechanically thinned source substrate to expose the crystal layer, wherein the area of ​​the etched and removed portion accounts for 5% to 30% of the total area of ​​the source substrate;

[0021] (5.3) Remove all remaining source substrate to completely expose the crystalline layer.

[0022] As an improvement of the above solution, in step (4), direct bonding is used to bond the transfer substrate to the bonding layer, and the bonding pressure is 5 kN to 15 kN.

[0023] As an improvement of the above scheme, the ε-Ga2O3 piezoelectric film layer is further annealed at a temperature of 200°C to 400°C for a time of 1h to 4h.

[0024] Correspondingly, the present invention also provides a gallium oxide piezoelectric substrate, which is prepared by the above-mentioned method for preparing the gallium oxide piezoelectric substrate.

[0025] The implementation of the present invention has the following beneficial effects:

[0026] The present invention first grows a crystal layer on a source substrate before growing an ε-Ga2O3 piezoelectric film layer, so that an ε-Ga2O3 film with uniform thickness and consistent crystal phase can be obtained, and then the ε-Ga2O3 piezoelectric film layer is combined with a transfer substrate through a substrate transfer technology. The crystal layer can be used as an etching stop layer to reduce the damage to the ε-Ga2O3 piezoelectric film layer caused by removing the source substrate. The gallium oxide piezoelectric substrate prepared by the present invention can meet the high quality requirements of small-size piezoelectric substrates, the thickness accuracy and uniformity in the ε-Ga2O3 piezoelectric film layer are good, the crystal phase consistency of the ε-Ga2O3 is high, and the prepared SAW resonator has better frequency selectivity and lower insertion loss than a traditional SAW resonator with LiTaO3 as a substrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a schematic diagram of the structure obtained after step S1 of an embodiment of the present invention;

[0028] Figure 2 It is a schematic diagram of the structure obtained after step S2 of an embodiment of the present invention.

[0029] Figure 3 This is a schematic diagram of the structure obtained after step S3 of an embodiment of the present invention;

[0030] Figure 4 This is a schematic diagram of the structure obtained after step S4 in an embodiment of the present invention;

[0031] Figure 5 This is a schematic diagram of the structure obtained after step S51 in an embodiment of the present invention;

[0032] Figure 6 This is a schematic diagram of the structure obtained after step S52 of an embodiment of the present invention;

[0033] Figure 7 This is a top view obtained after step S52 in an embodiment of the present invention;

[0034] Figure 8 This is a schematic diagram of the structure obtained after step S53 of the embodiment of the present invention;

[0035] Fig. 9 This is a schematic diagram of the structure obtained after step S6 in an embodiment of the present invention;

[0036] Fig.10 This is a TEM test result diagram of Example 3 of the present invention;

[0037] Fig.11 The XRD test result diagrams of Examples 1 to 3 of the present invention are shown;

[0038] Fig.12 is the gallium oxide film thickness data of Example 3 of the present invention;

[0039] Fig.13 Impedance data of a gallium oxide resonator and a LiTaO3 resonator according to Example 3 of the present invention (red line: gallium oxide resonator; blue line: LiTaO3 resonator). DETAILED DESCRIPTION

[0040] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in further detail below.

[0041] The present invention provides a method for preparing a gallium oxide piezoelectric substrate, comprising the following steps:

[0042] S1 . Provide a source substrate 1 , and prepare a crystalline layer 2 on the source substrate 1 .

[0043] Specifically, the substrate material is one or more of silicon carbide, sapphire, glass, and silicon. Preferably, the substrate is made of high resistivity zone melting silicon wafer, and the crystal orientation requirement is <111> The silicon material in this crystal orientation has hexagonal symmetry and can be used as a heteroepitaxial substrate for ε-Ga2O3 with a hexagonal crystal structure.

[0044] The material of the crystal layer is aluminum nitride and / or silicon carbide, which is generally a material with a small thermal expansion coefficient. Preferably, the thermal expansion coefficient of the crystal layer material is 4.5×10 -6 / ℃~5.5×10 -6 / ℃, by controlling the thermal expansion coefficient of the crystal layer material, the thermal mismatch between the gallium oxide material and the substrate material is alleviated. The thickness of the crystal layer is 5nm to 100nm, exemplified by 5nm, 10nm, 20nm, 50nm, 80nm or 100nm, but not limited to this. If the thickness of the crystal layer is less than 5nm, the effect of alleviating the crystal mismatch is weak; if the thickness of the crystal layer is greater than 100nm, it will cause the crystal quality to deteriorate. In addition, when a silicon substrate is selected as the source substrate, it is easy to generate amorphous silicon oxide with poor consistency on the surface of the silicon substrate in the early stage of gallium oxide epitaxial growth, which seriously reduces the quality of the subsequently grown gallium oxide film. Therefore, by epitaxially growing a high-quality gallium oxide film through the crystal layer, the obtained ε-Ga2O3 piezoelectric film has good thickness uniformity and high crystal phase consistency, thereby improving the consistency and reliability of the device.

[0045] S2, preparing an ε-Ga2O3 piezoelectric thin film layer 3 on the crystalline layer 2.

[0046] The thickness of the ε-Ga2O3 piezoelectric film layer is 100nm to 1000nm. If the piezoelectric film layer is too thin, it may not provide sufficient structural support, affecting the mechanical stability and durability of the device; if the piezoelectric film layer is too thick, it may cause increased loss of sound waves during propagation. Exemplarily, the thickness of the ε-Ga2O3 piezoelectric film layer is 100nm, 200nm, 300nm, 500nm, 800nm ​​or 1000nm, but not limited thereto.

[0047] Specifically, the ε-Ga2O3 piezoelectric thin film layer is prepared by MOCVD, and the growth temperature is 400°C to 600°C, and 400°C, 420°C, 450°C, 500°C, 550°C or 600°C are exemplary, but not limited thereto. The growth pressure of the ε-Ga2O3 piezoelectric thin film layer is 50mbar to 150mbar, and 50mbar, 60mbar, 80mbar, 100mbar, 120mbar or 150mbar are exemplary, but not limited thereto.

[0048] Since the ε-Ga2O3 piezoelectric film layer is grown by MOCVD, the growth temperature is relatively high, which will cause thermal mismatch with the source substrate, thereby causing greater stress in the piezoelectric film. In one embodiment, the ε-Ga2O3 piezoelectric film layer is further annealed at a temperature of 200°C to 400°C, exemplarily 200°C, 220°C, 250°C, 300°C, 350°C or 400°C, but not limited thereto. The annealing time is 1h to 4h, exemplarily 1h, 1.5h, 2h, 2.5h, 3h or 4h, but not limited thereto.

[0049] S3, preparing a bonding layer 4 on the ε-Ga2O3 piezoelectric film layer 3.

[0050] The bonding layer is usually made of insulating material, and may be made of one or more of silicon dioxide, silicon nitride, silicon oxynitride or silicon carbide, with a thickness of 1 μm to 10 μm.

[0051] In one embodiment, if the bonding layer has poor roughness, a surface polishing process may be performed by CMP.

[0052] S4. Provide a transfer substrate 5, and bond the ε-Ga2O3 piezoelectric thin film layer 3 to the transfer substrate 5 via the bonding layer 4.

[0053] The material of the transfer substrate is one or more of silicon carbide, sapphire, glass, and silicon. Preferably, the transfer substrate is a high resistivity zone melting silicon wafer with a crystal orientation requirement of <111> .

[0054] Specifically, direct bonding is used to bond the transfer substrate to the bonding layer, the bonding pressure is 5 kN to 15 kN, and the bonding is performed at room temperature to avoid generating large thermal stress.

[0055] S5 , thinning and etching the source substrate 1 to expose the crystal layer 2 .

[0056] Specifically, the following steps are included:

[0057] S51 , mechanically thinning the source substrate 1 , wherein the thickness of the source substrate after mechanical thinning is 10 μm to 100 μm.

[0058] S52, using photolithography and dry etching to partially etch the mechanically thinned source substrate 1 to expose the crystal layer 2, and the area of ​​the etched and removed portion accounts for 5% to 30% of the total area of ​​the source substrate. If the proportion of the area of ​​the etched and removed portion to the total area of ​​the source substrate is too small, it is not conducive to improving the stress release effect; if the proportion of the area of ​​the etched and removed portion to the total area of ​​the source substrate is too large, it will cause the wafer after the substrate is peeled off to warp, crack, etc., resulting in a decrease in the quality of the wafer.

[0059] In one embodiment, the etched removed portion is evenly distributed on the source substrate, which is conducive to uniform stress release. Specifically, the etched removed portion can be a plurality of evenly distributed concave portions of the same shape, or a ring concentric with the wafer, and the width and number of the ring can be set according to actual conditions.

[0060] S53, using photolithography and dry etching to completely remove the remaining source substrate 1, completely exposing the crystal layer 2, and realizing the stripping of the source substrate.

[0061] S6. Use wet etching or dry etching to remove the crystalline layer 2 to expose the ε-Ga2O3 piezoelectric thin film layer 3, and obtain a gallium oxide piezoelectric substrate. The crystalline layer can not only improve the quality of the ε-Ga2O3 piezoelectric thin film layer grown on the source substrate, but also serve as an etching stop layer during the source substrate peeling process to avoid damage to the ε-Ga2O3 piezoelectric thin film layer during the etching and peeling process of the substrate.

[0062] The present invention first grows a crystal layer on a source substrate before growing an ε-Ga2O3 piezoelectric film layer, and obtains an ε-Ga2O3 film with uniform thickness and consistent crystal phase by controlling the thermal expansion coefficient of the crystal layer material and the thickness of the crystal layer. The ε-Ga2O3 piezoelectric film layer is then combined with the transfer substrate through a substrate transfer technology. The crystal layer can also serve as an etching stop layer to reduce damage to the ε-Ga2O3 piezoelectric film layer caused by removing the source substrate. The gallium oxide piezoelectric substrate prepared by the present invention can meet the high quality requirements of small-size piezoelectric substrates.

[0063] The present invention will be further described in detail below with reference to specific embodiments.

[0064] Example 1

[0065] An embodiment of the present invention provides a method for preparing a gallium oxide piezoelectric substrate, comprising the following steps:

[0066] S1. Provide a Si substrate, and prepare a SiC crystalline layer on the Si substrate.

[0067] Specifically, the Si substrate uses high resistivity zone melting silicon wafers, and the crystal orientation requirements are <111> The thickness of the SiC crystal layer is 5 nm.

[0068] S2. Prepare an ε-Ga2O3 piezoelectric thin film layer on the SiC crystal layer.

[0069] The ε-Ga2O3 piezoelectric thin film layer was prepared by MOCVD at a growth temperature of 400°C and a growth pressure of 50 mbar. The thickness of the ε-Ga2O3 piezoelectric thin film layer was 100 nm.

[0070] S3. Prepare a SiO2 bonding layer on the ε-Ga2O3 piezoelectric film layer with a thickness of 1 μm, and perform surface polishing by CMP.

[0071] S4. Provide a transfer substrate, and directly bond the ε-Ga2O3 piezoelectric film layer to the transfer substrate through a SiO2 bonding layer. The bonding temperature is 80° C. and the bonding pressure is 15 kN.

[0072] The transfer substrate is selected from high resistivity zone melting silicon wafers, and the crystal orientation requirements <111> .

[0073] S5. Mechanically thinning and etching the source substrate to expose the crystalline layer.

[0074] Specifically, the following steps are included:

[0075] S51 . Mechanically thinning the source substrate. The thickness of the source substrate after mechanical thinning is 10 μm.

[0076] S52. Partially etch the mechanically thinned source substrate using photolithography and dry etching to expose the crystal layer. The etched and removed portion is a plurality of identical columnar structures evenly distributed. The area of ​​the etched and removed portion accounts for 5% of the total area of ​​the source substrate.

[0077] S53, using photolithography and dry etching to completely remove the remaining source substrate and expose the crystalline layer completely.

[0078] S6. Remove the crystal layer by wet etching or dry etching to expose the ε-Ga2O3 piezoelectric film layer, and obtain a gallium oxide piezoelectric substrate.

[0079] Example 2

[0080] An embodiment of the present invention provides a method for preparing a gallium oxide piezoelectric substrate, comprising the following steps:

[0081] S1. Provide a Si substrate, and prepare a SiC crystalline layer on the Si substrate.

[0082] Specifically, the Si substrate uses high resistivity zone melting silicon wafers, and the crystal orientation requirements are <111> The thickness of the SiC crystal layer is 20 nm.

[0083] S2. Prepare an ε-Ga2O3 piezoelectric thin film layer on the SiC crystal layer.

[0084] The ε-Ga2O3 piezoelectric thin film layer was prepared by MOCVD at a growth temperature of 500°C and a growth pressure of 100 mbar. The thickness of the ε-Ga2O3 piezoelectric thin film layer was 450 nm.

[0085] S3. Prepare a SiO2 bonding layer on the ε-Ga2O3 piezoelectric film layer with a thickness of 6 μm, and perform surface polishing by CMP.

[0086] S4. Provide a transfer substrate, and directly bond the ε-Ga2O3 piezoelectric film layer to the transfer substrate through a SiO2 bonding layer. The bonding temperature is 90° C. and the bonding pressure is 8 kN.

[0087] The transfer substrate is selected from high resistivity zone melting silicon wafers, and the crystal orientation requirements <111> .

[0088] S5. Mechanically thinning and etching the source substrate to expose the crystalline layer.

[0089] Specifically, the following steps are included:

[0090] S51 . Mechanically thinning the source substrate. The thickness of the source substrate after mechanical thinning is 40 μm.

[0091] S52. Partially etch the source substrate after mechanical thinning by photolithography and dry etching to expose the crystal layer. The etched and removed portion is three circular ring structures with the same width and concentric with the wafer. The area of ​​the etched and removed portion accounts for 25% of the total area of ​​the source substrate.

[0092] S53, using photolithography and dry etching to completely remove the remaining source substrate, and completely expose the crystal layer. S6, using wet etching or dry etching to remove the crystal layer, and expose the ε-Ga2O3 piezoelectric film layer, and obtain a gallium oxide piezoelectric substrate.

[0093] Example 3

[0094] The embodiment of the present invention provides a method for preparing a gallium oxide piezoelectric substrate, which differs from the embodiment 3 in that after the ε-Ga2O3 piezoelectric film layer is grown by MOCVD, the ε-Ga2O3 piezoelectric film layer is annealed at a temperature of 300°C for 2 hours. The rest is the same as the embodiment 3.

[0095] The piezoelectric substrates obtained in Examples 1 to 3 were prepared into SAW resonators under the same process and their performance was tested. Fig.10 and Fig.11 It can be seen that the samples have good crystal quality, the atomic lattice arrangement is clear, and the selected area electron diffraction pattern also shows that the samples are ε-phase gallium oxide. The XRD results can confirm that the samples are all ε-Ga2O3 on silicon substrates, without β-phase stability problems, and only the (004) orientation of different diffraction orders is measured, indicating good crystal orientation consistency. Fig.12 It can be seen that the thickness of the substrate formed based on ε-Ga2O3 piezoelectric thin film material is easier to control, and CMP is not required for film thickness adjustment. The formed film layer has better accuracy and uniformity, and the cost is lower. Fig.13 It can be seen that, compared with the conventional SAW resonator with LiTaO3 as the substrate, the SAW resonator prepared by the present invention has a higher quality factor, and accordingly, has better frequency selectivity and lower insertion loss.

[0096] The above is a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the present invention. These improvements and modifications are also considered to be within the scope of protection of the present invention.

Claims

1. A method for preparing a gallium oxide piezoelectric substrate, It is characterized in that The following steps are involved: (1) providing a source substrate and preparing a crystalline layer on the source substrate; (2) Preparation of ε-Ga on the crystalline layer 2 O 3 Piezoelectric film layer; (3) In the ε-Ga 2 O 3 preparing a bonding layer on the piezoelectric film layer; (4) Provide a transfer substrate and bond the ε-Ga 2 O 3 The piezoelectric film layer is bonded to the transfer substrate; (5) thinning and etching the source substrate to expose the crystalline layer; (6) Remove the crystal layer to expose ε-Ga 2 O 3 The piezoelectric film layer is formed to obtain a gallium oxide piezoelectric substrate.

2. The method for preparing the gallium oxide piezoelectric substrate according to claim 1, It is characterized in that The material of the crystal layer is aluminum nitride and / or silicon carbide, and the thickness is 5nm-100nm.

3. The method for preparing the gallium oxide piezoelectric substrate according to claim 1, It is characterized in that The ε-Ga 2 O 3 The thickness of the piezoelectric thin film layer is 100 nm to 1000 nm.

4. The method for preparing the gallium oxide piezoelectric substrate according to claim 1, It is characterized in that The ε-Ga was prepared by metal organic chemical vapor deposition. 2 O 3 The piezoelectric thin film layer has a growth temperature of 400°C to 600°C.

5. The method for preparing the gallium oxide piezoelectric substrate according to claim 1, It is characterized in that The bonding layer is made of one or more of silicon dioxide, silicon nitride, silicon oxynitride, and silicon carbide, and has a thickness of 1 μm to 10 μm.

6. The method for preparing the gallium oxide piezoelectric substrate according to claim 1, It is characterized in that The material of the substrate is one or more of silicon carbide, sapphire, glass, and silicon; The material of the transfer substrate is one or more of silicon carbide, sapphire, glass, and silicon.

7. The method for preparing the gallium oxide piezoelectric substrate according to claim 1, It is characterized in that Step (5) comprises the following steps: (5.1) Mechanically thinning the source substrate, wherein the thickness of the source substrate after mechanical thinning is 10 μm to 100 μm; (5.2) Partially etching the mechanically thinned source substrate to expose the crystal layer, wherein the area of ​​the etched and removed portion accounts for 5% to 30% of the total area of ​​the source substrate; (5.3) Remove all remaining source substrate to completely expose the crystalline layer.

8. The method for preparing the gallium oxide piezoelectric substrate according to claim 1, It is characterized in that In step (4), direct bonding is used to bond the transfer substrate to the bonding layer, and the bonding pressure is 5 kN to 15 kN.

9. The method for preparing the gallium oxide piezoelectric substrate according to claim 1, It is characterized in that Also includes ε-Ga 2 O 3 The piezoelectric film layer is annealed at a temperature of 200° C. to 400° C. for a time of 1 h to 4 h.

10. A gallium oxide piezoelectric substrate, It is characterized in that The gallium oxide piezoelectric substrate is prepared by the method for preparing a gallium oxide piezoelectric substrate according to any one of claims 1 to 9.

Citation Information

Cited By

  • Epsilon-phase gallium oxide thin film, preparation method thereof and semiconductor device