C-Co3O4 catalyst as well as preparation method and application thereof
The carbon-containing Co3O4 catalyst prepared by the sol-gel method solves the problem of insufficient PCDD/Fs degradation technology in the steel industry, achieves efficient degradation of chlorobenzene and toluene, and provides efficient, economical and environmentally friendly catalytic oxidation solutions.
Patent Information
- Application Number
- CN202410933580.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-15
AI Technical Summary
The existing environmental equipment in the steel industry is difficult to fully meet the ultra-low emission limit requirements, especially the lack of degradation technology for PCDD/Fs, and there are challenges in designing high-performance catalysts in catalytic combustion methods.
The carbon-containing Co3O4 catalyst is prepared by a simple sol-gel method. By changing the air calcining temperature, a highly efficient C-Co3O4 catalyst is prepared for catalytic oxidation of volatile organic compounds chlorobenzene and toluene to achieve their high levels at lower temperatures. Conversion degradation.
It has achieved efficient degradation of parachlorobenzene and toluene, significantly improved conversion rate, and the catalyst can be reused, with excellent reaction stability and environmental protection, and is suitable for industrial applications.
Smart Images

Figure CN118949989A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a C-Co3O4 catalyst and a preparation method and application thereof, belonging to the field of waste gas purification and catalytic oxidation catalyst preparation. Background Art
[0002] The coal-based energy structure of the steel industry makes pollution and carbon from the same source and has large emissions. Pollution and carbon emissions rank first in the industrial industry. At present, one of the three major challenges facing the steel industry in achieving the coordinated development goals of pollution reduction and carbon reduction is to reduce carbon in pollution control, that is, it is necessary to iteratively upgrade the existing ultra-low emission technology to reduce the carbon increment in the whole life cycle caused by high energy consumption and material consumption. Studies have shown that polychlorinated dibenzo-p-dioxins and polychlorinated dibenzofurans (hereinafter referred to as PCDD / Fs) are recognized by the World Health Organization as a first-class carcinogen for humans, with "three-cause" (teratogenic, carcinogenic, mutagenic) toxicity. According to statistics, about 90% of PCDD / Fs, the main gaseous pollutants produced in the steel production process, are produced in the sintering process. Therefore, more stringent standards and requirements are proposed for the emission of pollutants in steel sintering flue gas. Flue gas recirculation and activated carbon adsorption can reduce PCDD / Fs and conventional pollutants (nitrogen oxides, sulfur dioxide, etc.), and are important technologies for reducing PCDD / Fs in sintering waste gas. However, due to the difficulty in treating PCDD / Fs, the existing environmental protection equipment and technology in the steel industry cannot fully meet the requirements of the latest ultra-low emission limits and lacks environmental protection equipment and technology specifically for PCDD / Fs degradation. At present, in actual industry, gas-solid process elimination is usually selected, such as thermal combustion, catalytic combustion (oxidation) and other technologies, to achieve the degradation and elimination of PCDD / Fs while treating other pollutants. For catalytic combustion, the design of high-performance catalysts is the key. At the same time, in recent years, the application of advanced oxidation processes (AOPs) to the removal of gaseous pollutants has attracted the attention of more and more researchers. In this process, active oxygen species can be produced by ultraviolet photolysis, heating or metal catalysis H2O2 or persulfate (PDS / PMS). Gaseous pollutants will be absorbed into the water phase, and active oxygen species can quickly oxidize volatile organic compounds. The intermediate products of degradation are usually more hydrophilic and most of them are captured in the water phase. Compared with gas-solid processes, AOPs degradation of VOCs (volatile organic compounds) can successfully avoid the release of toxic byproducts into the atmospheric environment, thereby significantly reducing secondary air pollution. It is particularly important to note that due to the complex structure and strong toxicity of dioxins, the analysis process is relatively complicated. Therefore, in the initial stage of laboratory research on catalysts, chlorobenzene compounds with a chemical structure similar to dioxins are usually selected to replace dioxins to evaluate the degradation activity and anti-poisoning performance of catalysts. The results show that chlorobenzene is the simplest chlorinated aromatic hydrocarbon, which is similar to dioxins in structure and can be used as a molecular model of chlorinated aromatic compounds to simulate the degradation activity of dioxin-type organic pollutants in the catalytic process, reaction kinetics calculations, and catalytic mechanism analysis.
[0003] Transition metal oxides represented by Co3O4 have many advantages, such as rich Co valence, unoccupied d orbital, strong redox performance, rich active oxygen, abundant resources, etc., and are therefore regarded as potential substitutes for precious metal catalysts. Therefore, the present invention selects a simple sol-gel method and prepares a series of Co3O4 catalysts by changing different air calcination temperatures for catalytic oxidation of PCDD / Fs (chlorobenzene as a model pollutant) and toluene in steel sintering flue gas.
[0004] The invention discloses a preparation method and application of chlorobenzene and toluene, a volatile organic compound, by catalytic oxidation of a carbon-containing Co3O4 catalyst. The invention provides a preparation method of a modified Co3O4 catalyst and a treatment method for efficiently removing multi-polluting gases (chlorobenzene and toluene) for industrial practical application of effectively removing chlorobenzene and toluene, a volatile organic compound, in a terminal treatment device (adsorption desorption + RTO / RCO, RTO refers to a regenerative thermal oxidation technology, and RCO refers to a regenerative catalytic combustion method). Summary of the invention
[0005] In order to prepare a simpler, more economical and more efficient new catalyst, one of the purposes of the present invention is to provide a method for preparing a C-Co3O4 catalyst, the preparation method comprising the following steps:
[0006] (1) Dissolve Co(NO3)2·6H2O in deionized water to obtain a cobalt nitrate aqueous solution.
[0007] (2) Dissolve citric acid in deionized water to obtain a citric acid aqueous solution.
[0008] (3) gradually adding the citric acid aqueous solution obtained in step (2) to the cobalt nitrate aqueous solution in step (1), stirring in a constant temperature water bath until the water is completely evaporated to obtain a pink xerogel.
[0009] (4) Drying the pink xerogel obtained in step (3) to obtain a fluffy xerogel.
[0010] (5) Grinding the fluffy dry gel obtained in step (4) into fine particles and calcining them in an air atmosphere to obtain a C-Co3O4 catalyst.
[0011] Preferably, the molar volume concentration of the cobalt nitrate aqueous solution in step (1) is 0.25 mol / L to 0.50 mol / L.
[0012] Preferably, the molar volume concentration of the citric acid aqueous solution in step (2) is 1 mol / L to 2 mol / L.
[0013] Preferably, in step (3), the volume ratio of the aqueous cobalt nitrate solution to the aqueous citric acid solution is 4:1; and the temperature of the constant temperature water bath is 80-100°C.
[0014] Preferably, in step (4), the drying temperature is 60 to 110° C. and the drying time is 12 to 24 hours.
[0015] Preferably, in step (5), the calcination temperature is 250-350° C. and the calcination time is 6-10 hours.
[0016] Another object of the present invention is to provide an application of a C-Co3O4 catalyst in the catalytic oxidation of volatile organic compounds.
[0017] Preferably, the reaction temperature of the C-Co3O4 catalyst in catalytic oxidation of volatile organic matter is 100-400°C, the reaction volume space velocity is 40,000-120,000 mL / (g·h), and the gas concentration of the volatile organic matter is 200-410 ppm.
[0018] Preferably, the volatile organic compounds are benzene series compounds, including chlorine-containing volatile organic compounds chlorobenzene and typical volatile organic compounds toluene.
[0019] Beneficial Effects of the Invention
[0020] (1) The present invention uses a simple sol-gel method to prepare the Co3O4 catalyst, providing a simple, efficient, low-energy, and low-cost method for synthesizing Co3O4. The method does not require the use of any surfactant, is environmentally friendly, and does not produce toxic or harmful byproducts.
[0021] (2) The preparation process of the Co3O4 catalyst provided by the present invention is easy to control and has a high yield, and is suitable for mass production in future industrial applications. It can achieve effective degradation of chlorine-containing volatile organic pollutants in the gas phase, such as chlorobenzene and toluene, and its conversion rate is significantly improved compared with commercial Co3O4 catalysts. At a relatively low temperature of 300°C, a conversion rate of nearly 90% for chlorobenzene and a conversion rate of nearly 100% for toluene can be achieved simultaneously, which is of great significance for environmental governance.
[0022] (3) The Co3O4 catalyst of the present invention has a simpler preparation method. A Co3O4 catalyst containing a certain amount of carbon (C) can be obtained without conventional hydrothermal crystallization or even air calcination at a relatively high temperature. It is found through testing that when chlorobenzene and toluene are completely converted at a relatively high temperature (315°C), the yield of CO2 is close to 100%, indicating that chlorobenzene and toluene can be completely mineralized at this temperature to generate non-toxic CO2. The present invention uses a C-containing Co3O4 catalyst to conduct a catalytic oxidation reaction, which can effectively degrade chlorobenzene and toluene, and is highly efficient, economical and environmentally friendly.
[0023] (4) The catalyst can be reused and has excellent reaction stability. Even if it is deactivated at low temperature (275°C) due to the accumulation of intermediates and the failure of chlorine-containing species to dissociate in time, the catalyst can be restored to its original reaction activity by raising the temperature under the original reaction atmosphere.
[0024] (5) The Co3O4 catalyst of the present invention can be used in the field of thermal catalysis and also has excellent chlorobenzene removal performance in the catalytic activation persulfate system in the field of advanced oxidation processes. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The performance diagram of catalytic oxidation of gas-phase chlorobenzene by the catalysts in Examples 1 to 3 and Comparative Examples 2 and 3 is shown.
[0026] Figure 2 This is a performance diagram of the catalytic oxidation of gas-phase chlorobenzene under different reaction space velocity conditions of the C-Co3O4-250 catalyst prepared in Example 1.
[0027] Figure 3 This is the performance diagram of catalytic oxidation of gas-phase chlorobenzene by C-Co3O4-250 prepared in Example 1 and Nano-Co3O4 (0.08 g) + AC (0.02 g) -M prepared in Comparative Example 1.
[0028] Figure 4 This is the performance diagram of removing gas-phase chlorobenzene by catalytic activation of PMS using two different C-Co3O4 catalysts prepared in Example 1 and Comparative Example 3.
[0029] Figure 5 This is a performance diagram of catalytic oxidation of gas-phase toluene by two different C-Co3O4 catalysts prepared in Example 1 and Comparative Example 3.
[0030] Figure 6 This is a performance diagram of the simultaneous catalytic oxidation of gas-phase chlorobenzene and toluene by two different C-Co3O4 catalysts prepared in Example 1, Example 2 and Comparative Example 3.
[0031] Figure 7 This is the performance diagram of the catalyst stability (53h) of the C-Co3O4-300 catalyst prepared in Example 2 for the simultaneous catalytic oxidation of gas-phase chlorobenzene and toluene at 295°C. DETAILED DESCRIPTION
[0032] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. However, the following embodiments are merely simple examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.
[0033] Example 1
[0034] A method for preparing a C-Co3O4 catalyst comprises the following steps:
[0035] (1) Weigh 0.02 mol of Co(NO3)2·6H2O and dissolve it in 80 mL of deionized water. Mix well by ultrasonication to obtain a cobalt nitrate aqueous solution (0.25 mol / L).
[0036] (2) Weigh 0.02 mol of citric acid and dissolve it in 20 mL of deionized water. Similarly, ultrasonic mixing is used to obtain a citric acid aqueous solution (1 mol / L).
[0037] (3) slowly adding the citric acid aqueous solution obtained in step (2) to the cobalt nitrate aqueous solution prepared in step (1), and then placing the mixture in a water bath at 80° C. and subjecting the mixture to magnetic stirring in a water bath until the water is completely evaporated to obtain a pink xerogel.
[0038] (4) The pink dry gel prepared in step (3) was placed in a constant temperature drying oven at 110° C. and dried for 12 h to obtain a fluffy dry gel.
[0039] (5) The fluffy dry gel obtained in step (4) was placed in a mortar and ground into fine particles, and then placed in a tubular calcination furnace and heated to 250°C at a heating rate of 5°C / min under air atmosphere and calcined at a constant temperature for 6 hours to obtain a C-Co3O4 catalyst, which was named C-Co3O4-250.
[0040] The C-Co3O4-250 prepared in this example is used to catalyze the oxidation of 200±10ppm gaseous chlorobenzene (C6H5Cl), and the specific steps are as follows:
[0041] (1) A nitrogen and oxygen balanced bubbling process was performed. Chlorobenzene (containing 11% oxygen) at a final relatively stable concentration of 200±10 ppm was introduced into the reaction equipment. When the gas concentration was stable, the volume flow rate of chlorobenzene per unit time was adjusted to 100 mL / min, and the reaction volume space velocity was adjusted to 60,000 mL / (g·h).
[0042] (2) After the catalyst C-Co3O4-250 adsorbed the reaction gas in step (1) until the adsorption was saturated, the activity test of the catalyst was carried out at 100-375°C, where each 25°C was a temperature interval, and data collection and testing were carried out after each temperature point was stabilized for 10-15 minutes. The results showed that as the temperature increased, the conversion rate of p-chlorobenzene showed a gradual increase trend, and a conversion rate of p-chlorobenzene of about 99% was achieved at 320°C. The results of the catalytic performance are shown in Figure 2. Figure 1 As shown, its T 50 (the temperature required to achieve 50% conversion) and T 90(The temperature required to achieve 90% conversion rate) is lower than that of commercial nano Co3O4 (297°C). In order to further compare the catalytic activity of C-Co3O4-250 at different space velocities, the catalytic activity evaluation was carried out at space velocities of 40,000 mL / (g·h) and 120,000 mL / (g·h). The results of the catalytic performance are shown in Figure 2. Figure 2 As shown in the figure, even at a higher space velocity of 120,000 mL / (g·h), a conversion rate of about 99% of p-chlorobenzene can still be achieved at 320°C. Therefore, it can be shown that the C-Co3O4-250 catalyst prepared by this method has advantages in catalytic oxidation removal of chlorobenzene, and lays the foundation for future practical applicability.
[0043] The C-Co3O4-250 catalyst prepared by the present invention is applied to catalytic activation of PMS to remove gaseous chlorobenzene. The obtained C-Co3O4-250 catalyst is used to catalytically activate PMS to treat 80±4ppm gaseous chlorobenzene (C6H5Cl), and the specific steps are as follows:
[0044] (1) 80±4ppm chlorobenzene (containing 10% oxygen) balanced by nitrogen and oxygen is introduced into the reactor, and the volume flow rate of chlorobenzene per unit time is adjusted to 0.7 times the volume of the reaction liquid (chlorobenzene gas flow rate is 0.5L / min). Stable concentration of chlorobenzene gas is introduced into the reaction liquid through the sand core plate in the reactor, and the gas is dispersed into small bubbles at the bottom of the reaction tank.
[0045] (2) After the reaction gas is stable, a certain amount of potassium persulfate is added to the aqueous solution, and the molar mass concentration of persulfate is adjusted to form a 10 mmol / L PMS aqueous solution. After the reaction gas and the persulfate aqueous solution are evenly mixed, the prepared C-Co3O4-250 catalyst with a mass concentration of 0.5 g / L is directly added to the reactor. At this time, the catalyst can quickly excite the persulfate in the water to form active species (such as hydroxyl radicals, sulfate radicals or singlet oxygen species formed by the catalyst / PMS coupling aqueous solution system). 1 O2, etc.).
[0046] (3) In the process of gas rising to the water surface, it can fully react with the active substances produced by the catalytic activation of the carbon catalyst, and be catalytically oxidized to produce CO2 or other related intermediate products; the generated CO2 gas is discharged from the reactor along with the gas, while the intermediate products that are not completely oxidized remain in the reaction liquid in the form of liquid. Subsequently, additional persulfate and catalyst need to be added to treat the reaction liquid until it meets the standards before discharge.
[0047] The result of the reaction is Figure 4As shown, the removal rate of chlorobenzene remained above 90% within three hours of reaction. Therefore, it can be explained that the C-Co3O4-250 catalyst prepared by this method not only has excellent thermal catalytic activity in thermal catalysis, but also has certain practical applicability in the liquid-phase PMS activation and removal of chlorobenzene.
[0048] The C-Co3O4-250 catalyst prepared in this example is used to catalytically oxidize 400±10ppm gaseous toluene (C6H5CH3). The specific application scenarios are as follows:
[0049] (1) Toluene (containing 11% oxygen) at a relatively stable concentration of 400±10 ppm was introduced into the reaction equipment by nitrogen and oxygen balance bubbling. When the gas concentration was stable, the toluene volume flow rate per unit time was adjusted to 100 mL / min and the reaction volume space velocity was 60,000 mL / (g·h).
[0050] (2) After the catalyst is adsorbed to saturation with the reaction gas of step (1), the activity test of the catalyst is conducted at 100-350°C, with 25°C as a temperature interval. Data collection and testing are conducted after each temperature point is stabilized for 10-15 minutes. The results show that as the temperature increases, the conversion rate of toluene shows a trend of gradual increase. At 240°C, a conversion rate of toluene of about 99% is achieved. The results of the catalytic performance are as follows: Figure 5 Therefore, it can be shown that the C-Co3O4-250 catalyst prepared by this method has advantages in catalytic oxidation removal of toluene, and lays the foundation for future practical applicability.
[0051] The C-Co3O4-250 catalyst prepared in this example is used to simultaneously catalyze the oxidation of 200±10ppm gaseous chlorobenzene (C6H5Cl) and 200±10ppm gaseous toluene (C6H5CH3). The specific steps are as follows:
[0052] (1) A nitrogen and oxygen balance bubbling process was performed by introducing 200±10 ppm chlorobenzene and 200±10 ppm toluene (containing 11% oxygen) at a relatively stable concentration into the reaction equipment. When the gas concentration was stable, the gas volume flow rate per unit time was adjusted to 100 mL / min and the reaction volume space velocity was 60,000 mL / (g·h).
[0053] (2) After the catalyst is adsorbed to saturation with the reaction gas of step (1), the activity test of the catalyst is conducted at 100-375°C, wherein each temperature interval is 25°C, and data collection and testing are conducted after each temperature point is stabilized for 10-15 minutes. The results show that with the increase of temperature, the conversion rate of chlorobenzene and toluene shows a trend of gradual increase, and the conversion rate of chlorobenzene is about 99% at 325°C, and the conversion rate of toluene is about 99% at 250°C. The results of the reaction are shown in Figure 6 (A) and (B), it can be shown that the C-Co3O4-250 catalyst prepared by this method has certain practical applicability in the simultaneous catalytic oxidation removal of chlorobenzene and toluene.
[0054] Example 2
[0055] A method for preparing a C-Co3O4 catalyst comprises the following steps:
[0056] (1) Weigh 0.02 mol of Co(NO3)2·6H2O and dissolve it in 80 mL of deionized water. Mix well by ultrasonication to obtain a cobalt nitrate aqueous solution (0.25 mol / L).
[0057] (2) Weigh 0.02 mol of citric acid and dissolve it in 20 mL of deionized water. Similarly, ultrasonic mixing is used to obtain a citric acid aqueous solution (1 mol / L).
[0058] (3) slowly adding the citric acid aqueous solution obtained in step (2) to the cobalt nitrate aqueous solution prepared in step (1), and then placing the mixture in a water bath at 80° C. and subjecting the mixture to magnetic stirring in a water bath until the water is completely evaporated to obtain a pink xerogel.
[0059] (4) The pink dry gel prepared in step (3) was placed in a constant temperature drying oven at 80° C. and dried for 16 h to obtain a fluffy dry gel.
[0060] (5) The fluffy dry gel obtained in step (4) was placed in a mortar and ground into fine particles, which were then placed in a tubular calcination furnace and heated to 300°C at a heating rate of 5°C / min in an air atmosphere and calcined at a constant temperature for 6 hours to obtain a C-Co3O4 catalyst, which was named C-Co3O4-300.
[0061] The C-Co3O4-300 prepared in this example is used to catalyze the oxidation of 200±10ppm gaseous chlorobenzene (C6H5Cl), and the specific steps are as follows:
[0062] (1) A nitrogen and oxygen balanced bubbling process was performed. Chlorobenzene (containing 11% oxygen) at a final relatively stable concentration of 200±10 ppm was introduced into the reaction equipment. When the gas concentration was stable, the volume flow rate of chlorobenzene per unit time was adjusted to 100 mL / min, and the reaction volume space velocity was adjusted to 60,000 mL / (g·h).
[0063] (2) After the catalyst C-Co3O4-300 was adsorbed with the reaction gas of step (1) until the adsorption was saturated, the activity test of the catalyst was carried out at 100-375°C, where 25°C was a temperature range, and data collection and testing were carried out after each temperature point was stabilized for 10-15 minutes. The results showed that with the increase of temperature, the conversion rate of p-chlorobenzene showed a trend of gradual increase, and the conversion rate of p-chlorobenzene was about 99% at 301°C. The results of catalytic performance are shown in Figure 2. Figure 1 As shown, its T 50 (the temperature required to achieve 50% conversion) and T 90 The temperature required to achieve 90% conversion is about 50°C and 29°C earlier than that of commercial nano-Co3O4 (258°C and 297°C), respectively. Therefore, it can be shown that the C-Co3O4 catalyst prepared by this method has advantages in catalytic oxidation removal of chlorobenzene, and lays the foundation for future practical applicability.
[0064] The C-Co3O4-300 catalyst prepared in this example is used to simultaneously catalyze the oxidation of 200±10ppm gaseous chlorobenzene (C6H5Cl) and 200±10ppm gaseous toluene (C6H5CH3). The specific steps are as follows:
[0065] (1) A nitrogen and oxygen balance bubbling process was performed by introducing 200±10 ppm chlorobenzene and 200±10 ppm toluene (containing 11% oxygen) at a relatively stable concentration into the reaction equipment. When the gas concentration was stable, the gas volume flow rate per unit time was adjusted to 100 mL / min and the reaction volume space velocity was 60,000 mL / (g·h).
[0066] (2) After the catalyst is adsorbed to saturation with the reaction gas of step (1), the activity test of the catalyst is conducted at 100-375°C, wherein each temperature interval is 25°C, and data collection and testing are conducted after each temperature point is stabilized for 10-15 minutes. The results show that with the increase of temperature, the conversion rate of chlorobenzene and toluene shows a trend of gradual increase, with a conversion rate of about 99% for chlorobenzene at 325°C and a conversion rate of about 97% for toluene at 250°C. The results of the reaction are shown in Figure 2. Figure 6 (A) and (B) show that the C-Co3O4-300 catalyst prepared by this method has certain practical applicability in the simultaneous catalytic oxidation removal of chlorobenzene and toluene.
[0067] The C-Co3O4-300 catalyst prepared in this example was used for stability test in the simultaneous catalytic oxidation of 200±10ppm gaseous chlorobenzene (C6H5Cl) and 200±10ppm gaseous toluene (C6H5CH3). The specific steps are as follows:
[0068] (1) The nitrogen and oxygen balanced bubbling was performed by introducing 200±10ppm chlorobenzene and 200±10ppm toluene (containing 11% oxygen) at a relatively stable concentration into the reaction equipment. When the gas concentration was stable, the gas volume flow rate per unit time was adjusted to 100mL / min and the reaction volume space velocity was 60,000mL / (g·h).
[0069] (2) After the catalyst is heated to 275°C, a stability test of the catalyst is performed, and after a period of time, the temperature is raised to 295°C for stability test. The results show that at 295°C, the conversion rates of chlorobenzene and toluene show a stable trend, and at 295°C, a conversion rate of nearly 90% for chlorobenzene and about 99% for toluene is achieved. The reaction results are as follows: Figure 7 As shown, it can be explained that the C-Co3O4-300 catalyst prepared by this method has certain practical applicability in the simultaneous catalytic oxidation removal of chlorobenzene and toluene.
[0070] Example 3
[0071] A method for preparing a C-Co3O4 catalyst comprises the following steps:
[0072] (1) Weigh 0.04 mol of Co(NO3)2·6H2O and dissolve it in 80 mL of deionized water. Mix well by ultrasonication to obtain a cobalt nitrate aqueous solution (0.5 mol / L).
[0073] (2) Weigh 0.04 mol of citric acid and dissolve it in 20 mL of deionized water. Similarly, ultrasonic mixing is used to obtain a citric acid aqueous solution (2 mol / L).
[0074] (3) slowly adding the citric acid aqueous solution obtained in step (2) to the cobalt nitrate aqueous solution prepared in step (1), and then placing the mixture in a water bath at 80° C. and subjecting the mixture to magnetic stirring in a water bath until the water is completely evaporated to obtain a pink xerogel.
[0075] (4) The pink xerogel prepared in step (3) was placed in a constant temperature drying oven at 60° C. and dried for 24 h to obtain a fluffy xerogel.
[0076] (5) The fluffy dry gel obtained in step (4) was placed in a mortar and ground into fine particles, and then placed in a tubular calcination furnace and heated to 350°C at a heating rate of 5°C / min in an air atmosphere and calcined at a constant temperature for 10 h to obtain a C-Co3O4 catalyst, which was named C-Co3O4-350.
[0077] The C-Co3O4-350 prepared in this example is used to catalyze the oxidation of 200±10ppm gaseous chlorobenzene (C6H5Cl), and the specific steps are as follows:
[0078] (1) A nitrogen and oxygen balanced bubbling process was performed. Chlorobenzene (containing 11% oxygen) at a final relatively stable concentration of 200±10 ppm was introduced into the reaction equipment. When the gas concentration was stable, the volume flow rate of chlorobenzene per unit time was adjusted to 100 mL / min, and the reaction volume space velocity was adjusted to 60,000 mL / (g·h).
[0079] (2) After the catalyst C-Co3O4-350 was adsorbed with the reaction gas of step (1) until adsorption saturation, the activity test of the catalyst was carried out at 100-375°C, wherein each temperature interval was 25°C, and data collection and testing were carried out after each temperature point was stabilized for 10-15 minutes. The results showed that with the increase of temperature, the conversion rate of p-chlorobenzene showed a trend of gradual increase, and the conversion rate of p-chlorobenzene was about 99% at 325°C. The results of catalytic performance are shown in Figure 1 As shown, its T 50 The temperature required to achieve 50% conversion is lower than that of commercial nano Co3O4 (258°C). Therefore, it can be shown that the C-Co3O4 catalyst prepared by this method has advantages in catalytic oxidation of chlorobenzene removal, and lays the foundation for future practical applicability.
[0080] Comparative Example 1
[0081] In order to prove that the C-Co3O4-250 catalyst prepared by the present invention has excellent catalytic oxidation performance of chlorobenzene, a commercial Nano-Co3O4+AC-M catalyst obtained by mechanically mixing commercial nano-Co3O4 (60-80 mesh) and activated coke (60-80 mesh) was selected for comparison of catalytic performance.
[0082] The commercial Nano-Co3O4+AC-M catalyst was used to catalytically oxidize 200±10ppm gaseous chlorobenzene (C6H5Cl). The specific steps are as follows:
[0083] (1) A relatively stable concentration of 200±10 ppm chlorobenzene (11% oxygen) was introduced into the reaction equipment by nitrogen and oxygen balance bubbling. After the gas concentration was stabilized, the volume flow rate of chlorobenzene per unit time was adjusted to 100 mL / min and the reaction volume space velocity was 60,000 mL / (g·h).
[0084] (2) After the catalyst was adsorbed to saturation with the reaction gas of step (1), the activity test of the catalyst was conducted at 100-375°C, wherein each 25°C was a temperature interval, and data collection and testing were conducted after each temperature point was stabilized for 10-15 minutes. The results showed that as the temperature increased, the conversion rate of p-chlorobenzene showed a trend of gradual increase, and about 100% conversion rate of p-chlorobenzene was achieved at 375°C. Its performance was worse than that of the C-Co3O4-250 catalyst prepared in Example 1. The results of its reaction were as follows: Figure 3 As shown. Therefore, it can be explained that the C-Co3O4 catalyst prepared by this method has advantages in the catalytic oxidation removal of chlorobenzene. The presence of C in the Co3O4 nanoparticles promotes the catalytic oxidation performance of chlorobenzene. The performance improvement cannot be achieved by simply mechanically mixing C and Co3O4. Therefore, the preparation of the C-Co3O4 catalyst lays the foundation for future practical applicability.
[0085] Comparative Example 2
[0086] A method for preparing a C-Co3O4 catalyst comprises the following steps:
[0087] (1) Weigh 0.02 mol of Co(NO3)2·6H2O and dissolve it in 80 mL of deionized water. Mix well by ultrasonication to obtain a cobalt nitrate aqueous solution (0.25 mol / L).
[0088] (2) Weigh 0.02 mol of citric acid and dissolve it in 20 mL of deionized water. Similarly, ultrasonic mixing is used to obtain a citric acid aqueous solution (1 mol / L).
[0089] (3) slowly adding the citric acid aqueous solution obtained in step (2) to the cobalt nitrate aqueous solution prepared in step (1), and then placing the mixture in a water bath at 80° C. and subjecting the mixture to magnetic stirring in a water bath until the water is completely evaporated to obtain a pink xerogel.
[0090] (4) The pink dry gel prepared in step (3) was placed in a constant temperature drying oven at 110° C. and dried for 6 h to obtain a fluffy dry gel.
[0091] (5) The fluffy dry gel obtained in step (4) was placed in a mortar and ground into fine particles, which were then placed in a tubular calcination furnace and heated to 400°C at a heating rate of 5°C / min in an air atmosphere and calcined at a constant temperature for 6 hours to obtain a C-Co3O4 catalyst, which was named C-Co3O4-400.
[0092] The C-Co3O4-400 prepared in this example is used to catalyze the oxidation of 200±10ppm gaseous chlorobenzene (C6H5Cl), and the specific steps are as follows:
[0093] (1) A nitrogen and oxygen balanced bubbling process was performed. Chlorobenzene (containing 11% oxygen) at a final relatively stable concentration of 200±10 ppm was introduced into the reaction equipment. When the gas concentration was stable, the volume flow rate of chlorobenzene per unit time was adjusted to 100 mL / min, and the reaction volume space velocity was adjusted to 60,000 mL / (g·h).
[0094] (2) After the catalyst C-Co3O4-400 was adsorbed with the reaction gas of step (1) until adsorption saturation, the activity test of the catalyst was carried out at 100-375°C, wherein each temperature interval was 25°C, and data collection and testing were carried out after each temperature point was stabilized for 10-15 minutes. The results showed that with the increase of temperature, the conversion rate of p-chlorobenzene showed a trend of gradual increase, and the conversion rate of p-chlorobenzene was about 99% at 325°C. The results of catalytic performance are shown in Figure 2. Figure 1 As shown, it is obvious that when the temperature is lower than 320°C, the catalytic effect is not as good as that of Example 1.
[0095] Comparative Example 3
[0096] A method for preparing a C-Co3O4 catalyst comprises the following steps:
[0097] (1) Weigh 0.02 mol of Co(NO3)2·6H2O and dissolve it in 80 mL of deionized water. Mix well by ultrasonication to obtain a cobalt nitrate aqueous solution (0.25 mol / L).
[0098] (2) Weigh 0.02 mol of citric acid and dissolve it in 20 mL of deionized water. Similarly, ultrasonic mixing is used to obtain a citric acid aqueous solution (1 mol / L).
[0099] (3) slowly adding the citric acid aqueous solution obtained in step (2) to the cobalt nitrate aqueous solution prepared in step (1), and then placing the mixture in a water bath at 80° C. and subjecting the mixture to magnetic stirring in a water bath until the water is completely evaporated to obtain a pink xerogel.
[0100] (4) The pink dry gel prepared in step (3) was placed in a constant temperature drying oven at 110° C. and dried for 12 h to obtain a fluffy dry gel.
[0101] (5) The fluffy dry gel obtained in step (4) was placed in a mortar and ground into fine particles, which were then placed in a tubular calcination furnace and heated to 450°C at a heating rate of 5°C / min in an air atmosphere and calcined at a constant temperature for 6 hours to obtain a C-Co3O4 catalyst, which was named C-Co3O4-450.
[0102] The C-Co3O4-450 catalyst prepared in this example is used to catalytically oxidize 200±10ppm gaseous chlorobenzene (C6H5Cl), and the specific steps are as follows:
[0103] (1) A nitrogen and oxygen balanced bubbling process was performed. Chlorobenzene (containing 11% oxygen) at a final relatively stable concentration of 200±10 ppm was introduced into the reaction equipment. When the gas concentration was stable, the volume flow rate of chlorobenzene per unit time was adjusted to 100 mL / min, and the reaction volume space velocity was adjusted to 60,000 mL / (g·h).
[0104] (2) After the catalyst C-Co3O4-450 was adsorbed with the reaction gas of step (1) until the adsorption was saturated, the activity test of the catalyst was carried out at 100-375°C, where 25°C was a temperature range, and data collection and testing were carried out after each temperature point was stabilized for 10-15 minutes. The results showed that with the increase of temperature, the conversion rate of p-chlorobenzene showed a trend of gradual increase, and the conversion rate of p-chlorobenzene was about 99% at 400°C. The results of catalytic performance are shown in Figure 1 Therefore, it can be shown that the C-Co3O4 catalyst prepared by this method has advantages in catalytic oxidation removal of chlorobenzene, and lays the foundation for future practical applicability.
[0105] The C-Co3O4-450 catalyst prepared in this example was used to catalytically activate PMS to treat 80±4ppm gaseous chlorobenzene (C6H5Cl). The specific steps are as follows:
[0106] (1) 80±4ppm chlorobenzene (10% oxygen) balanced by nitrogen and oxygen is introduced into the reactor, and the volume flow rate of chlorobenzene per unit time is adjusted to 0.7 times the volume of the reaction liquid (chlorobenzene gas flow rate is 0.5L / min). Stable concentration of chlorobenzene gas is introduced into the reaction liquid through the sand core plate in the reactor, and the gas is dispersed into small bubbles at the bottom of the reaction tank.
[0107] (2) After the reaction gas is stable, a certain amount of potassium persulfate is added to the aqueous solution, and the molar mass concentration of persulfate is adjusted to form a 10 mmol / L PMS aqueous solution. After the reaction gas and the persulfate aqueous solution are evenly mixed, the prepared C-Co3O4-450 catalyst with a mass concentration of 0.5 g / L is directly added to the reactor. At this time, the catalyst can quickly excite the persulfate in the water to form active species (such as hydroxyl radicals, sulfate radicals or singlet oxygen species formed by the catalyst / PMS coupling aqueous solution system). 1 O2, etc.).
[0108] (3) In the process of gas rising to the water surface, it can fully react with the active substances produced by the catalytic activation of the carbon catalyst, and be catalytically oxidized to produce CO2 or other related intermediate products; the generated CO2 gas is discharged from the reactor along with the gas, while the intermediate products that are not completely oxidized remain in the reaction liquid in the form of liquid. Subsequently, additional persulfate and catalyst need to be added to treat the reaction liquid until it meets the standards before discharge.
[0109] The result of the reaction is Figure 4 As shown, the removal rate of chlorobenzene is maintained above 60% within three hours of reaction, which indicates that the catalyst prepared in this comparative example is not as good as that in Example 1.
[0110] The C-Co3O4-450 catalyst prepared in this example is used to catalytically oxidize 400±10ppm gaseous toluene (C6H5CH3). The specific application scenarios are as follows:
[0111] (1) The reaction equipment was introduced with nitrogen and oxygen balanced bubbling to produce 400±10 ppm toluene (11% oxygen) at a relatively stable concentration. When the gas concentration was stable, the volume flow rate of chlorobenzene per unit time was adjusted to 100 mL / min and the reaction volume space velocity to 60,000 mL / (g·h).
[0112] (2) After the catalyst was adsorbed to saturation with the reaction gas of step (1), the activity test of the catalyst was conducted at 100-350°C, wherein 25°C was a temperature interval, and data collection and testing were conducted after each temperature point was stabilized for 10-15 minutes. The results showed that as the temperature increased, the conversion rate of toluene showed a trend of gradual increase, and about 99% conversion rate of toluene was achieved at 275°C. It can be seen that its conversion efficiency is not as good as that of Example 1. The results of catalytic performance are shown in FIG. Figure 5 Therefore, it can be shown that the catalyst prepared in this example is not as good as that in Example 1 in terms of catalytic oxidation removal of toluene.
[0113] The C-Co3O4-450 catalyst prepared in this embodiment is used to simultaneously catalyze the oxidation of 200±10ppm gaseous chlorobenzene (C6H5Cl) and 200±10ppm gaseous toluene (C6H5CH3), and the specific steps are as follows:
[0114] (1) The nitrogen and oxygen balanced bubbling was performed by introducing 200±10ppm chlorobenzene and 200±10ppm toluene (11% oxygen) at a relatively stable concentration into the reaction equipment. When the gas concentration was stable, the gas volume flow rate per unit time was adjusted to 100mL / min and the reaction volume space velocity was 60,000mL / (g·h).
[0115] (2) After the catalyst is adsorbed to saturation with the reaction gas of step (1), the activity test of the catalyst is conducted at 100-375°C, wherein 25°C is a temperature interval, and data collection and testing are conducted after each temperature point is stabilized for 10-15 minutes. The results show that as the temperature increases, the conversion rates of p-chlorobenzene and toluene show a trend of gradual increase, with a conversion rate of about 99% for p-chlorobenzene achieved at 325°C and a conversion rate of about 99% for toluene achieved at 250°C. The reaction results are as follows: Figure 6 As shown in (A) and (B), it can be seen that the catalytic effect of the catalyst prepared in this comparative example is not as good as that of Example 1 and Example 2.
Claims
1. A method for preparing a C-Co3O4 catalyst, characterized in that: The preparation method comprises the following steps: (1) dissolving Co(NO3)2·6H2O in deionized water to obtain a cobalt nitrate aqueous solution; (2) dissolving citric acid in deionized water to obtain a citric acid aqueous solution; (3) gradually adding the citric acid aqueous solution obtained in step (2) dropwise to the cobalt nitrate aqueous solution in step (1), and stirring in a constant temperature water bath until the water is completely evaporated to obtain a pink xerogel; (4) drying the pink xerogel obtained in step (3) to obtain a fluffy xerogel; (5) Grinding the fluffy dry gel obtained in step (4) into fine particles and calcining them in an air atmosphere to obtain a C-Co3O4 catalyst.
2. The method for preparing the C-Co3O4 catalyst according to claim 1, characterized in that: The molar volume concentration of the cobalt nitrate aqueous solution in step (1) is 0.25 mol / L to 0.50 mol / L.
3. The method for preparing the C-Co3O4 catalyst according to claim 1, characterized in that: The molar volume concentration of the citric acid aqueous solution in step (2) is 1 mol / L to 2 mol / L.
4. The method for preparing the C-Co3O4 catalyst according to claim 1, characterized in that: In step (3), the volume ratio of the cobalt nitrate aqueous solution to the citric acid aqueous solution is 4:1; and the temperature of the constant temperature water bath is 80-100°C.
5. The method for preparing the C-Co3O4 catalyst according to claim 1, characterized in that: In step (4), the drying temperature is 60 to 110° C. and the drying time is 12 to 24 hours.
6. The method for preparing the C-Co3O4 catalyst according to claim 1, characterized in that: In step (5), the calcination temperature is 250-350° C. and the calcination time is 6-10 hours.
7. Use of the C-Co3O4 catalyst prepared by the method according to any one of claims 1 to 6 in catalytic oxidation of volatile organic compounds.
8. The use according to claim 7, characterized in that: The volatile organic compounds are benzene compounds, including chlorobenzene, a chlorine-containing volatile organic compound, and toluene, a volatile organic compound containing a benzene ring.
Citation Information
Patent Citations
Nucleocapsid energizing agent for propelling agent and method for preparing same
CN101549289A
Co-based supported catalyst for catalytic removal of benzene-series compounds in air and preparation method thereof
CN103191743A
Carbon-coated cobalt oxide and simple controllable preparation method thereof
CN104843804A
Catalyst applied to low temperature catalytic combustion of chlorination aromatic hydrocarbon as well as preparation method and application thereof
CN106994348A
Efficient compounding method for chain-like carbon nanospheres
CN107089651A