Special vehicle fender reinforcing rib friction stir welding method

Through the friction stir welding welding method, the combination of overlap structure and anti-spill positioning blocks solves the problems of low strength and large deformation after welding of special vehicle fenders, and achieves high-quality and beautiful welding effects.

CN118951291APending Publication Date: 2024-11-15BEIJING NORTH VEHICLE GROUP CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411313316.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The strength of the special vehicle fenders is low after welding and the deformation is too large, which cannot meet the product usage requirements.

Method used

Friction stir welding welding method is adopted. First weld the middle part of the reinforcement rib through the lap structure, and then weld both ends. Use anti-spill positioning blocks to prevent the overflow of aluminum alloy material, and control the process parameters of friction stir welding such as rotation speed, feed speed and Depression volume.

Benefits of technology

Effectively control the welding deformation of aluminum alloy thin plates, improve welding quality and processability, enhance the strength and appearance of the fenders, and solve the deformation problems that traditional argon arc welding cannot solve.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118951291A_ABST
    Figure CN118951291A_ABST
Patent Text Reader

Abstract

According to the friction stir welding method for the reinforcing rib of the fender of the special vehicle, a stirring head with a stirring needle larger than the thickness of an upper-layer plate is used for achieving penetrating friction stir welding of an aluminum alloy thin plate in a lap joint mode. According to the welding method, welding deformation of the aluminum alloy sheet can be effectively controlled, the welding quality and welding manufacturability of welding seams are improved, the welding quality and use requirements of the fender are guaranteed, the technical bottleneck that welding deformation of the large aluminum alloy sheet is too large is broken through, and the welding quality and appearance of an aluminum alloy product are greatly improved. By means of the method, the conventional aluminum alloy friction stir welding mode can be expanded, and the problems which cannot be solved through a traditional argon arc welding method are effectively solved. According to the welding method, the welding sequence of the middle and the two ends and the clamping method for preventing plastic overflow of the aluminum alloy are adopted, the welding precision of the workpiece can be improved, the plastic deviation of the strip-shaped aluminum alloy product in the friction stir welding process is effectively controlled, and meanwhile the problem of plastic overflow of the aluminum alloy material after stirring is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of welding, and in particular relates to a friction stir welding method for fender reinforcement ribs of a special vehicle aluminum alloy plate overlapped in the form ... friction stir welding method. Background Art

[0002] The fender is an important part of the special vehicle protection components, which has the function of protecting the special vehicle tracks and beautifying the appearance. In terms of performance requirements, it is required to play the role of protecting the tracks and have considerable strength, and it is also required to be light and beautiful. Therefore, it is necessary to adopt a structure with thin aluminum alloy plates and welded stiffeners. In the process of scientific research and trial production, after welding by argon arc welding, due to the thin aluminum plate and large deformation, it cannot meet the product use requirements. Therefore, it is necessary to combine the structural form of the stiffener and the fender overlap, and design a stir friction welding penetration welding method, using the stirring needle of the stirring head to penetrate the stiffener foot plate and stir friction welding with the fender body. Summary of the invention

[0003] 1. Technical issues to be resolved

[0004] The invention provides a friction stir welding method for a fender reinforcement rib of a special vehicle, so as to solve the technical problems that the fender of the special vehicle has low strength and is excessively deformed after being welded with the reinforcement rib.

[0005] (II) Technical solution

[0006] In order to solve the above technical problems, the present invention proposes a special vehicle fender reinforcement stir friction welding method. The reinforcement and the fender body adopt an overlap structure, first clamp the two ends of the reinforcement, weld the middle part, and then weld the welds at both ends.

[0007] Furthermore, the fender is made of aluminum alloy LY21, and the thickness is 3 mm.

[0008] Furthermore, the material of the reinforcing rib is aluminum alloy LY21, and the thickness of the reinforcing rib foot plate is 3 mm.

[0009] Furthermore, a stirring head is used whose stirring needle is larger than the thickness of the reinforcing rib foot plate.

[0010] Furthermore, a 4 mm stirring needle was used.

[0011] Furthermore, an anti-overflow positioning block is used on the outer side of the reinforcing rib foot plate to prevent the aluminum alloy material from being squeezed and overflowed after plastic deformation.

[0012] Furthermore, the length of the reinforcing rib is 500-700 mm, and the number of the intermittent welds is 3-4 sections.

[0013] Furthermore, when a 4mm stirring head is selected, the welding contact surface is Φ12mm and the stirring needle length is 4mm.

[0014] Furthermore, the welding speed of the friction stir welding is 1200 r / m and the feed speed is 100 mm / min.

[0015] Furthermore, the downward pressure of the friction stir welding is 0.2 mm, the starting delay is 6 to 10 s, the ending delay is 6 to 10 s, and the welding inclination angle is 2.5°.

[0016] (III) Beneficial effects

[0017] The present invention proposes a friction stir welding method for the reinforcement ribs of the fender of a special vehicle, which uses a stirring head with a stirring needle larger than the thickness of the upper plate to achieve penetration friction stir welding of overlapping aluminum alloy thin plates. The welding method can effectively control the welding deformation of the aluminum alloy thin plate, improve the welding quality and welding processability of the weld, ensure the welding quality and use requirements of the fender, break through the technical bottleneck of excessive welding deformation of large aluminum alloy thin plates, and greatly improve the welding quality and appearance of aluminum alloy products. The method can expand the conventional friction stir welding form of aluminum alloys and effectively solve the problems that cannot be solved by traditional argon arc welding methods. The welding sequence of first the middle and then the two ends and the clamping method to prevent the plastic overflow of the aluminum alloy adopted by the present invention can improve the welding accuracy of the workpiece, effectively control the plastic deviation of the long strip-shaped aluminum alloy product during the friction stir welding process, and avoid the problem of plastic overflow of the aluminum alloy material after stirring, improve the weld quality and external appearance, and ensure product consistency. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1a This is a front view of a fender of a special vehicle targeted by the present invention. Figure 1b It is a top view;

[0019] Figure 2a This is the front view of the reinforcing rib targeted by the present invention, Figure 2b is a side view;

[0020] Figure 3 It is a schematic diagram of the overlapping structure of the fender and the reinforcing rib in the present invention;

[0021] Figure 4 It is a schematic diagram of the stirring head penetration welding in the present invention.

[0022] Figure 5 It is a schematic diagram of the welding sequence and clamping position in the present invention;

[0023] Figure 6a This is a front view of the fender reinforcement welding in the present invention. Figure 6b This is a top view. DETAILED DESCRIPTION

[0024] In order to make the purpose, content and advantages of the present invention more clear, the specific implementation methods of the present invention are further described in detail below in conjunction with the drawings and examples.

[0025] The special vehicle fender targeted by the present invention is made of aluminum alloy LY21, with a thickness of 3 mm. The product is thin, has a large width, and has low strength. Figure 1a and 1b As shown in 2a and 2b, it is easy to deform and needs to be welded with reinforcing ribs to improve its overall rigidity. The reinforcing rib material is aluminum alloy LY21, and the structure is shown in 2a and 2b. It is formed by stamping to improve the product strength.

[0026] In view of the welding quality requirements and process structure characteristics of the fender and the stiffener, the welding process adopts stir friction welding. Therefore, this embodiment proposes a special vehicle fender stiffener friction welding method. According to the welding structure characteristics that the stiffener foot plate and the fender body are both 3mm aluminum alloy thin plates, the overlap structure and the characteristics of the aluminum alloy thin plate are used to design the overlap penetration welding. The overlap structure of the fender 1 and the stiffener 2 is as follows: Figure 3 As shown in FIG. 1 , a stirring head (4 mm stirring needle) with a stirring needle larger than the thickness of the reinforcing rib foot plate is used to penetrate the reinforcing rib foot plate to achieve penetration stir friction welding of the overlapped aluminum alloy thin plate, such as Figure 4 By selecting a suitable stirring head 3 to determine the width of the reinforcing rib foot plate, the fitting portion between the reinforcing rib and the fender body can be increased. Under the premise of a slight increase in weight (0.8 kg per piece), the post-welding strength is greatly improved, the implementation requirements of the new process are met, and the welding deformation is better controlled.

[0027] There is a certain welding pressure during the friction stir welding process. The aluminum alloy will produce fluidity after local plasticization. When clamping, it is necessary to control the welding deformation of the aluminum alloy plate and the overflow of the material from the penetrated upper foot plate to the outside. Therefore, when performing the friction stir welding method, considering that the length of the reinforcement rib is 500-700mm, the intermittent welds are designed into 3-4 sections. The two ends of the reinforcement rib are clamped first, and the middle part is welded to avoid the inconsistency of the plastic deformation of the fender body and the reinforcement rib to produce a gap in the assembly fitting; then the welds at both ends are welded, and the outer side of the reinforcement rib foot plate is fixed. By using the anti-overflow positioning block 4, the aluminum alloy material is prevented from being squeezed and overflowing after plastic deformation. Figure 5 As shown, the excessive plastic deformation of aluminum alloy materials during welding can be effectively controlled to ensure welding size and quality.

[0028] In this embodiment, the specific process parameters of friction stir welding are: 4mm stirring head, welding contact surface of Φ12mm, stirring needle length of 4mm; welding speed of 1200r / m, feed speed of 100mm / min, downward pressure of 0.2mm, start delay of 6-10s, end delay of 6-10s, welding inclination of 2.5°. Figure 6a and 6b shown.

[0029] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A friction stir welding method for fender reinforcement of special vehicles, characterized in that: The friction stir welding method is that the reinforcing rib and the fender body adopt an overlap structure, first clamp the two ends of the reinforcing rib, weld the middle part, and then weld the welds at the two ends.

2. The friction stir welding method for special vehicle fender reinforcement according to claim 1, characterized in that: The fender is made of aluminum alloy LY21 with a thickness of 3mm.

3. The friction stir welding method for special vehicle fender reinforcement according to claim 1, characterized in that: The material of the reinforcement rib is aluminum alloy LY21, and the thickness of the reinforcement rib foot plate is 3mm.

4. The friction stir welding method for special vehicle fender reinforcement according to claim 1, characterized in that: Use a stirring head with a stirring needle that is larger than the thickness of the reinforcement foot plate.

5. The friction stir welding method for special vehicle fender reinforcement according to claim 4, characterized in that: Use 4mm stirring needle.

6. The friction stir welding method for special vehicle fender reinforcement according to claim 1, characterized in that: On the outside of the reinforcing rib foot plate, an anti-overflow positioning block is used to prevent the aluminum alloy material from being squeezed and overflowing after plastic deformation.

7. The friction stir welding method for special vehicle fender reinforcement according to claim 1, characterized in that: The length of the reinforcement rib is 500-700 mm, and the intermittent welds are 3-4 sections.

8. The friction stir welding method for special vehicle fender reinforcement according to claim 1, characterized in that: When a 4mm stirring head is selected, the welding contact surface is Φ12mm and the stirring needle length is 4mm.

9. The friction stir welding method for special vehicle fender reinforcement according to claim 1, characterized in that: The welding speed of friction stir welding is 1200r / m and the feed speed is 100mm / min.

10. The friction stir welding method for special vehicle fender reinforcement according to claim 1, characterized in that: The downward pressure of the friction stir welding is 0.2 mm, the starting delay is 6 to 10 s, the ending delay is 6 to 10 s, and the welding inclination angle is 2.5°.