Preparation method of carbon aerogel wave-absorbing material based on self-foaming derivation of guar gum

Through the combined preparation method of guar gum and Zn(NO3)2·6H2O, a carbon aerogel absorbing material with a three-dimensional honeycomb pore structure was constructed, which solved the problems of complex process, high cost and pore wall thickness in the existing technology, and realized the problem of "complexity in the process", which was a good idea. The material's efficient electromagnetic wave absorption performance is achieved.

CN118954475AActive Publication Date: 2024-11-15HARBIN INST OF TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411028230.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

The existing carbon aerogel absorbing materials have complex preparation processes, high usage costs, thick pore walls, and mismatched impedances, which limits the improvement of material performance and application promotion.

Method used

Using the preparation method based on self-foaming and derivatization of guar gum, the combination of Zn(NO3)2·6H2O and guar gum is combined to form a hydrogel and freeze drying and high-temperature calcination to construct a three-dimensional honeycomb pore structure to regulate electromagnetic characteristics. .

Benefits of technology

It realizes the raw materials of the material, the preparation process is simple, the hole wall is thin and the structure is complete, which significantly improves the wave absorption performance of electromagnetic waves, especially in the 2-18GHz frequency band.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954475A_ABST
    Figure CN118954475A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of electromagnetic wave absorbing materials, in particular to a preparation method of a carbon aerogel wave absorbing material based on guar gum self-foaming derivation. The technical problems that carbon aerogel formed through a common technology is tedious in step, high in use cost, thick in hole wall and mismatched in impedance are solved. Comprising the following steps: 1, dissolving Zn (NO3) 2.6 H2O in deionized water, and adding guar gum to prepare hydrogel, 2, standing the hydrogel at room temperature, and carrying out freeze drying to obtain an aerogel precursor, 3, carrying out high-temperature calcination on the precursor to obtain aerogel, and 4, putting the aerogel into a hydrochloric acid solution, standing, washing, and drying to obtain the aerogel. The guar gum-derived carbon aerogel wave-absorbing material is obtained. The used raw materials are economical and easy to obtain, the preparation process is simple, the obtained product is thin in pore wall, light in weight and good in double-three-dimensional porous structure, meanwhile, the multiple reflection loss of electromagnetic waves in the wave-absorbing agent is enhanced, and the wave-absorbing performance is excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electromagnetic wave absorbing materials, and in particular to a method for preparing a carbon aerogel absorbing material derived from guar gum self-foaming. Background Art

[0002] In recent years, with the rapid development of wireless electronic communication technology, high-frequency electronic and communication equipment have been more widely used, which has caused serious electromagnetic pollution problems. Studies have shown that excessive electromagnetic waves will not only cause a certain degree of interference to some high-precision instruments, seriously affect the reliability of data, and hinder the progress of society, but also excessive electromagnetic radiation will have different degrees of impact on human health. For example, it interferes with the normal physiological functions of cells and organs, stimulates the nervous system, and then affects the immune system. These problems cannot be ignored.

[0003] In recent years, carbon aerogel materials, especially polymer-derived carbon, have become extremely competitive in absorbing materials due to their light weight, adjustable intrinsic conductivity and scalable production. However, a comprehensive analysis of the progress of related work shows that there are still some problems that need to be solved in the existing mainstream carbon aerogel absorbing materials. These include complex preparation processes, high use costs, and thick pore walls. The existence of these problems not only limits the further improvement of the performance of carbon aerogel absorbing materials, but also hinders their promotion in practical applications. In this case, the preparation of carbon aerogel absorbing materials with controllable microstructures through simple methods is still a key and difficult point in this field. Summary of the invention

[0004] The purpose of the research and development of the present invention is to solve the technical problems of cumbersome steps, high cost of use, thick pore wall and impedance mismatch in the formation of carbon aerogels by common technology, and to realize the construction of a three-dimensional honeycomb pore structure on the inner wall based on the original aerogel, so that its electromagnetic properties can be easily regulated and have good wave absorption performance within 2-18GHz. A brief overview of the present invention is given below to provide a basic understanding of certain aspects of the present invention. It should be understood that this overview is not an exhaustive overview of the present invention. It is not intended to determine the key or important parts of the present invention, nor is it intended to limit the scope of the present invention.

[0005] The technical solution of the present invention:

[0006] The preparation method of carbon aerogel absorbing material derived from guar gum self-foaming comprises the following steps:

[0007] Step 1: dissolving Zn(NO3)2·6H2O in deionized water, stirring evenly to obtain a transparent solution, then adding guar gum to the transparent solution, stirring until the mixture is evenly mixed, and preparing a hydrogel;

[0008] Step 2: placing the hydrogel at room temperature and freeze-drying it to obtain an aerogel precursor;

[0009] Step 3: placing the aerogel precursor in a porcelain boat and calcining it at high temperature in an argon atmosphere in a tubular furnace to obtain a black aerogel;

[0010] Step 4: Place the aerogel in a hydrochloric acid solution and let it stand, then wash it with deionized water and anhydrous ethanol, and then dry it in an oven to obtain a guar gum-derived carbon aerogel absorbing material.

[0011] Preferably, in step 1, the amount of Zn(NO3)2·6H2O is 1.5 g, the amount of deionized water is 100 mL, and the amount of guar gum is 1 g.

[0012] Preferably, the stirring temperature in step 1 is 35° C. and the stirring time is 10 min.

[0013] Preferably, the standing time of the hydrogel in step 2 is 48 hours, and the freeze-drying process is to place the standing hydrogel in an environment of -18°C, freeze it for 12 hours, and then put it into a freeze dryer and vacuum dry it at -57°C for 72 hours.

[0014] Preferably, the mass of the aerogel precursor in step 3 is 0.6 g.

[0015] Preferably, in step 3, the high temperature calcination process is to control the tubular furnace to heat up at a rate of 5°C / min to 800°C, and the calcination time is 2 hours.

[0016] Preferably, in step 4, the concentration of the hydrochloric acid solution is 4 mol / L, the volume of the hydrochloric acid solution is 30 mL, and the standing time is 12 hours.

[0017] The present invention has the following beneficial effects:

[0018] The guar gum-derived carbon aerogel absorbing material prepared by the present invention uses economical and readily available raw materials, has a simple preparation process, has a relatively thin pore wall, and has a complete and uniform three-dimensional structure of the obtained product.

[0019] The guar gum-derived carbon aerogel absorbing material prepared by the present invention has a good dual three-dimensional porous structure, which enhances the multiple reflection loss of electromagnetic waves inside the absorbing agent;

[0020] The guar gum-derived carbon aerogel wave-absorbing material prepared by the invention has thin thickness, light weight and excellent wave-absorbing performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is the scanning electron microscope image of the guar gum derived carbon aerogel absorber and the comparative sample;

[0022] Figure 2 is the XRD pattern of guar gum derived carbon aerogel absorber and the comparative sample;

[0023] Figure 3 It is the Raman spectra of guar gum derived carbon aerogel absorber and comparison sample;

[0024] Figure 4 is the real part curve of dielectric constant of guar gum derived carbon aerogel absorber and comparison sample;

[0025] Figure 5 is the imaginary part curve of dielectric constant of guar gum derived carbon aerogel absorber and comparison sample;

[0026] Figure 6 is the wave impedance curve of guar gum derived carbon aerogel absorber and comparison sample;

[0027] Figure 7 is a loss factor curve of guar gum derived carbon aerogel absorber and a comparative sample;

[0028] Figure 8 This is a graph of the electromagnetic wave absorption performance of guar gum derived carbon aerogel absorber.

[0029] Figure 1 a is a scanning electron microscope image of the comparison sample, and b is a scanning electron microscope image of the guar gum-derived carbon aerogel absorber. After the introduction of Zn(NO3)2·6H2O, a three-dimensional honeycomb pore structure appears on the inner wall of the aerogel layer, and the pore wall becomes thinner, the pore size becomes larger, Figure 2 Curve a in the middle is the XRD of the comparative sample, and curve b is the XRD of the guar gum derived carbon aerogel absorber. By comparing the X-ray diffraction standard card, it can be seen that the carbon aerogel prepared in Example 1 and the comparative sample are mainly composed of amorphous carbon. Figure 3 Curve a is the Raman spectrum of the comparative sample; curve b is the Raman spectrum of the guar gum derived carbon aerogel absorber. D / I G The values ​​are the same, which is mainly due to the fact that their carbonization temperature and carbonization time are the same. Figure 4 Curve a is the real part curve of the dielectric constant of the comparison sample; curve b is the real part curve of the guar gum derived carbon aerogel absorbing material. The real part value of the dielectric constant of the guar gum derived carbon aerogel absorbing material is higher than the real part value of the dielectric constant of the comparison sample. This is because the introduction of zinc nitrate increases the pore volume, increases the porosity, and reduces the volume density. The sample per unit mass is more likely to build a conductive network in the paraffin matrix under the action of an external electromagnetic field, thereby effectively improving the transmission efficiency of electrons. Figure 5The center line a is the imaginary part curve of the dielectric constant of the comparison sample; curve b is the imaginary part curve of the dielectric constant of the graphitized gradient hollow carbon / cobalt microsphere absorber. The imaginary part value of the dielectric constant of the guar gum-derived carbon aerogel absorber is higher than that of the comparison sample. This is because the introduction of zinc nitrate increases the pore volume, increases the porosity, and reduces the volume density. The sample per unit mass is easy to build a conductive network in the paraffin matrix under the action of an external electromagnetic field, thereby improving the material's conductivity, Figure 6 a is the wave impedance curve of the comparison sample; b is the wave impedance curve of the guar gum derived carbon aerogel absorber. The wave impedance value of the guar gum derived carbon aerogel absorber is lower than that of the comparison sample, indicating that the impedance matching characteristics of the material are improved by constructing a three-dimensional honeycomb pore structure on the inner wall. Figure 7 Curve a in the middle is the loss factor curve of the comparison sample; curve b is the loss factor curve of the guar gum derived carbon aerogel absorber. The loss capacity of the comparison sample is not as strong as that of the guar gum derived carbon aerogel absorber, indicating that the loss capacity of the material can be regulated by constructing a three-dimensional honeycomb pore structure on the inner wall. Figure 8 Figure a is a three-dimensional reflection loss diagram, and Figure b is a two-dimensional reflection loss diagram. The minimum reflection loss of the guar gum-derived carbon aerogel prepared in Example 1 reaches -25.5 dB at 18.0 GHz, and its effective absorbing bandwidth reaches 5.8 GHz, with a thickness of 1.8 mm. The frequency band range in which its reflection loss is less than -10 dB is approximately 4.0 to 18.0 GHz (approximately 14 GHz), which can achieve C-band, X-band and Ku-band coverage, indicating that the guar gum-derived carbon aerogel absorbing material has excellent electromagnetic wave absorption capability. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is described below by the specific embodiments shown in the accompanying drawings. However, it should be understood that these descriptions are only exemplary and are not intended to limit the scope of the present invention. In addition, in the following description, the description of well-known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.

[0031] Specific implementation method 1: Combination Figure 1-Figure 8 The present embodiment is described. The preparation method of the carbon aerogel absorbing material derived from guar gum self-foaming in the present embodiment comprises the following steps:

[0032] Step 1: dissolving Zn(NO3)2·6H2O in deionized water, stirring evenly to obtain a transparent solution, then adding guar gum to the transparent solution, stirring until the mixture is evenly mixed, and preparing a hydrogel;

[0033] Step 2: placing the hydrogel at room temperature and freeze-drying it to obtain an aerogel precursor;

[0034] Step 3: placing the aerogel precursor in a porcelain boat and calcining it at high temperature in an argon atmosphere in a tubular furnace to obtain an aerogel;

[0035] Step 4: Place the aerogel in a hydrochloric acid solution and let it stand, then wash it with deionized water and anhydrous ethanol, and then dry it in an oven to obtain a guar gum-derived carbon aerogel absorbing material.

[0036] Specific implementation method 2: Combination Figure 1-Figure 8 This embodiment describes the method for preparing a carbon aerogel absorbing material derived from guar gum self-foaming. In step 1, the amount of Zn(NO3)2·6H2O is 1.5 g, the amount of deionized water is 100 mL, and the amount of guar gum is 1 g.

[0037] Specific implementation method three: Combination Figure 1-Figure 8 The present embodiment is described. In the method for preparing the carbon aerogel absorbing material derived from guar gum self-foaming, the stirring temperature in step 1 is 35° C. and the stirring time is 10 min, which helps to promote sufficient cross-linking and make it more evenly dispersed.

[0038] Specific implementation method four: Combination Figure 1-Figure 8 The present embodiment is described. In the method for preparing a carbon aerogel absorbing material derived from guar gum self-foaming, the hydrogel in step 2 is allowed to stand for 48 hours, and the freeze-drying process is to place the hydrogel after standing at -18°C for 12 hours, and then put it into a freeze dryer for vacuum drying at -57°C for 72 hours.

[0039] Specific implementation method five: Combination Figure 1-Figure 8 This embodiment is described. In the method for preparing the carbon aerogel absorbing material derived from guar gum self-foaming described in this embodiment, the mass of the aerogel precursor in step three is 0.6 g.

[0040] Specific implementation method six: Combination Figure 1-Figure 8 The present embodiment is described. In the preparation method of the carbon aerogel absorbing material derived from guar gum self-foaming described in the present embodiment, the high temperature calcination process in step 3 is to control the tubular furnace to heat up at a rate of 5°C / min to 800°C, and the calcination time is 2 hours to ensure that it has the expected porous and carbonized properties.

[0041] Specific implementation method seven: Combination Figure 1-Figure 8 This embodiment describes the method for preparing a carbon aerogel absorbing material derived from guar gum self-foaming. In step 4, the hydrochloric acid solution is 4 mol / L, the volume of the hydrochloric acid solution is 30 mL, and the standing time is 12 hours to ensure that the metallic zinc is completely removed.

[0042] The guar gum derived carbon aerogel absorbing material prepared by the present invention has a maximum reflection loss of -25.5 dB. When the thickness of the absorber is 1.8 mm, the bandwidth in which the reflection loss is less than -10 dB can reach about 5.8 GHz, ranging from 12.2 to 18.0 GHz.

[0043] Embodiment 1

[0044] Dissolve 1.5 g Zn(NO3)2·6H2O in 100 mL deionized water and stir to obtain a transparent solution. Then add 1 g guar gum and stir to obtain a hydrogel.

[0045] The hydrogel was placed at room temperature for 48 hours, and then the hydrogel was frozen at -18°C for 12 hours, and then placed in a freeze dryer for vacuum drying at -57°C for 72 hours to obtain an aerogel precursor;

[0046] The aerogel precursor was placed in a porcelain boat and calcined at high temperature in a tubular furnace under an argon atmosphere. The heating rate of the tubular furnace was 5°C / min, the calcination temperature was 800°C, and the calcination time was 2 hours. After calcination, black aerogel was obtained.

[0047] The black aerogel was placed in a 30 mL hydrochloric acid solution with a concentration of 4 mol / L and allowed to stand for 24 hours. After standing, the aerogel was washed with deionized water and anhydrous ethanol. After washing, the aerogel was placed in a drying oven to dry. After drying, a guar gum-derived carbon aerogel absorbing material was obtained.

[0048] The comparative sample was prepared without adding Zn(NO3)2·6H2O in step 1, and other conditions were the same as those in Example 1.

[0049] It should be noted that in the above embodiments, as long as the technical solutions are not contradictory, they can be arranged and combined, and those skilled in the art can exhaust all possibilities based on the mathematical knowledge of arrangement and combination. Therefore, the present invention will no longer describe the technical solutions after arrangement and combination one by one, but it should be understood that the technical solutions after arrangement and combination have been disclosed by the present invention.

[0050] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. Preparation method of carbon aerogel absorbing material derived from guar gum self-foaming, It is characterized in that The steps include: Step 1: Zn(NO 3 ) 2 6H 2 O was dissolved in deionized water and stirred to obtain a transparent solution, and then guar gum was added to the transparent solution and stirred until the mixture was uniform to obtain a hydrogel; Step 2: placing the hydrogel at room temperature and freeze-drying it to obtain an aerogel precursor; Step 3: placing the aerogel precursor in a porcelain boat and calcining it at high temperature in an argon atmosphere in a tubular furnace to obtain a black aerogel; Step 4: Place the aerogel in a hydrochloric acid solution and let it stand, then wash it with deionized water and anhydrous ethanol, and then dry it in an oven to obtain a guar gum-derived carbon aerogel absorbing material.

2. The method for preparing the carbon aerogel absorbing material derived from guar gum self-foaming according to claim 1, Features: In step 1, Zn(NO 3 ) 2 6H 2 The amount of O is 1.5 g, the amount of deionized water is 100 mL, and the amount of guar gum is 1 g.

3. The method for preparing the carbon aerogel absorbing material derived from guar gum self-foaming according to claim 1, Features: In the step 1, the stirring temperature is 35° C. and the stirring time is 10 min.

4. The method for preparing the carbon aerogel absorbing material derived from guar gum self-foaming according to claim 1, Features: In step 2, the hydrogel is allowed to stand for 48 hours, and the freeze-drying process is to place the hydrogel after standing at -18°C for 12 hours, and then put it into a freeze dryer for vacuum drying at -57°C for 72 hours.

5. The method for preparing the carbon aerogel absorbing material derived from guar gum self-foaming according to claim 1, Features: The mass of the aerogel precursor in step 3 is 0.6 g.

6. The method for preparing the carbon aerogel absorbing material derived from guar gum self-foaming according to claim 1, Features: In step 3, the high temperature calcination process is to control the tubular furnace to heat up at a rate of 5°C / min to 800°C, and the calcination time is 2 hours.

7. The method for preparing the carbon aerogel absorbing material derived from guar gum self-foaming according to claim 1, Features: In step 4, the concentration of the hydrochloric acid solution is 4 mol / L, the volume of the hydrochloric acid solution is 30 mL, and the standing time is 12 hours.

Citation Information

Patent Citations

  • Cobalt-loaded Nb2CTx / carbon aerogel as well as preparation method and application thereof

    CN116099463A

  • Preparation method of novel three-dimensional porous biomass-derived carbon aerogel

    CN117756093A

  • Preparation method of three-dimensional porous carbon foam wave-absorbing material for packaging ultra-small Mo2C particles

    CN117985719A

  • Method of manufacturing eco-friendly and environmentally friendly carbon aerogel

    KR1020160127853A