Porous moisture absorption gel as well as preparation method and application thereof

By using ternary polymerizable eutectic solvents to prepare porous hygroscopic gels, the problems of stable dose and complex internal phase removal in traditional gel preparation are solved, and efficient hygroscopic performance and simple preparation process are achieved. They are suitable for atmospheric water collection and soil Improvement and other fields.

CN118955793AActive Publication Date: 2024-11-15SHANDONG UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411015682.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

The existing hygroscopic gels require a large number of stabilizers and complex internal phase removal processes during the preparation process, which limits their universality and hygroscopic properties, and the eutectic solvent polymer lacks flexibility and efficient hygroscopic properties.

Method used

Using ternary polymerizable eutectic solvents as the external phase, combined with biocompatible stabilizers and easy-dry organic solvents, porous absorbent gels are prepared through simple mixing, heating and vacuum drying processes to form a highly interpenetrating porous structure. The preparation process is simplified and the hygroscopic ability is improved.

Benefits of technology

It has achieved porous hygroscopic gels with high porosity, low density and large specific surface area, which significantly improves the effects of atmospheric water collection, soil improvement and humidity monitoring. The preparation process is simple and economical, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955793A_ABST
    Figure CN118955793A_ABST
Patent Text Reader

Abstract

The invention relates to the field of atmospheric environment water collection, in particular to porous moisture absorption gel as well as a preparation method and application thereof. The preparation method comprises the following steps: firstly, carrying out structure modification on a traditional binary eutectic solvent to prepare a ternary eutectic solvent with hygroscopicity and polymerizability, taking the ternary eutectic solvent as an external phase and an organic solvent which is easy to dry and remove as an internal phase, and preparing a high-internal-phase emulsion under the assistance of a stabilizer in a proper proportion; and continuing to add an initiator and a cross-linking agent to form a template pre-polymerization solution, and carrying out subsequent polymerization and vacuum drying to prepare the porous moisture absorption gel. The high internal phase emulsion is used as a template, and a highly interpenetrating porous structure can be introduced for the gel, so that the mass transfer process of water molecules is accelerated, and the atmospheric water collection effect is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of atmospheric environmental water collection, and in particular to a porous hygroscopic gel and a preparation method and application thereof. Background Art

[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] The atmosphere contains a large amount of fresh water, with an estimated water content of 12,900 km3, accounting for about 10% of the fresh water resources on Earth, and can be continuously replenished through the water cycle. Therefore, adsorption-based atmospheric water harvesting systems are considered to be a very promising method to alleviate water shortages. Such systems can achieve fresh water production in a wide range of relative humidity (RH), especially in low RH (RH < 60%) environments by directly using adsorbents with high water affinity to capture water molecules from the air to produce fresh water. In the process of adsorption-based atmospheric water harvesting, the hygroscopic agent is a key factor that determines the overall performance of the adsorbent material and the applicable environmental conditions.

[0004] A hygroscopic agent is a material with a high affinity for water molecules, which can capture water molecules in the atmosphere and enrich them on the surface or in the internal structure. Its hygroscopic mechanism can be divided into: surface water adsorption, micropore filling, capillary condensation, and absorption depending on the hygroscopic agent. Currently, commonly used hygroscopic materials include nanoporous materials (MOF, COF, and microporous aluminum phosphate, etc.), hygroscopic salts (lithium chloride, lithium bromide, and calcium chloride, etc.), highly hydrophilic polymers, and liquid hygroscopic agents. Among them, gel materials have gradually become an ideal atmospheric hygroscopic material due to their unique hydrophilicity and swelling properties. For example, Wang et al. (R. Wang, et al. ACS Materials Lett. 2020, 2, 471.) further doped lithium chloride hygroscopic agent into the hydrogel formed by sodium alginate and calcium chloride to achieve the collection of atmospheric water under low energy consumption. In addition, the introduction of lithium chloride can increase the degree of cross-linking to improve the mechanical properties of the gel, thereby improving the cyclic stability of the gel. Chen et al. (T. Chen, et al. Angew. Chem. Int. Ed. 2020, 59, 19237.) soaked the hydrogel formed by polymethacrylic acid and polyacrylamide in glycerol and used solvent replacement to prepare super hygroscopic organic hydrogel.

[0005] Currently, most hygroscopic gels are hydrogels or organic hydrogels, and there is limited research on eutectic solvent gels (Eutectogels) constructed with a low eutectic solvent as a dispersion medium that has a lower saturated vapor pressure and more efficient hygroscopic properties. Summary of the invention

[0006] In order to overcome the above problems, the present invention provides a porous hygroscopic gel and a preparation method and application thereof. The present invention firstly performs structural modification on the traditional binary low eutectic solvent to prepare a ternary low eutectic solvent with both hygroscopicity and polymerizability, and uses this as the external phase, and an organic solvent that is easy to dry and remove as the internal phase, and prepares a high internal phase emulsion with the assistance of a suitable proportion and a stabilizer; then, an initiator and a cross-linking agent are added to form a template prepolymer liquid, and a porous hygroscopic gel is prepared through subsequent polymerization and vacuum drying processes. Using a high internal phase emulsion as a template can introduce a highly interpenetrating porous structure into the gel, thereby accelerating the mass transfer process of water molecules and realizing the atmospheric water collection effect.

[0007] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:

[0008] The first aspect of the present invention provides a porous absorbent gel composition comprising the following components:

[0009] A ternary polymerizable deep eutectic solvent, composed of a monomer, a hydrogen bond acceptor and a hydrogen bond donor;

[0010] Stabilizers;

[0011] internal phase;

[0012] Initiator;

[0013] Cross-linking agent;

[0014] Accelerator.

[0015] The second aspect of the present invention provides a porous absorbent gel, which is formed from the above-mentioned porous absorbent gel composition into a high internal phase emulsion gel and the internal phase is removed to form a porous structure with high porosity.

[0016] The third aspect of the present invention provides a method for preparing the porous hygroscopic gel, comprising the following steps:

[0017] (1) mixing a monomer, a hydrogen bond acceptor, and a hydrogen bond donor and heating them to form a ternary polymerizable low eutectic solvent;

[0018] (2) adding a stabilizer and an internal phase to the ternary polymerizable low eutectic solvent in (1), and obtaining a high internal phase emulsion after homogenization;

[0019] (3) continuing to add initiator, crosslinker and accelerator to the high internal phase emulsion in (2), homogenously mixing to form a template prepolymer solution, initiating external phase polymerization, and obtaining a high internal phase emulsion gel;

[0020] (4) Removing the internal phase from the high internal phase emulsion gel, a porous hygroscopic gel is obtained.

[0021] The fourth aspect of the present invention provides the use of the porous hygroscopic gel as a self-hygroscopic material in atmospheric water collection.

[0022] A fifth aspect of the present invention provides use of the porous hygroscopic gel as a self-hygroscopic material in humidity monitoring.

[0023] A sixth aspect of the present invention provides use of the porous hygroscopic gel as a self-hygroscopic material in soil improvement.

[0024] The beneficial effects of the present invention are:

[0025] (1) Traditional high internal phase emulsions often require the addition of a large amount of stabilizers to ensure their emulsification effect during the preparation process, and the amount of polymerizable monomers added in the external phase is limited, which seriously limits the universality of the gel preparation method and is not conducive to the improvement of mechanical properties and hygroscopic capacity. The ternary polymerizable low eutectic solvent proposed in the present invention can simultaneously play the role of reactive monomer, reaction medium and hygroscopic component in the preparation process of porous hygroscopic materials. Biocompatible amphiphilic proteins are used as stabilizers to reduce the amount of stabilizers used, and are green and environmentally friendly. In the preparation process, only simple homogenization is required to form a stable high internal phase emulsion, with low energy consumption and easy operation.

[0026] (2) Compared with the traditional high internal phase emulsion template method, the present invention uses a ternary low eutectic solvent with both hygroscopicity and polymerizability as the external phase and an organic solvent that is easily removed by drying as the internal phase. A porous hygroscopic gel can be prepared through a simple mixing, heating, and vacuum drying process. A highly interpenetrating porous structure can be formed without the need for a complex internal phase removal process, and the structure and properties of the porous gel can be changed by adjusting the template parameters.

[0027] (3) The porous hygroscopic gel prepared by the present invention has high porosity (59.5%), low density (0.7 g / cm 3 ), large specific surface area (37.5m 2 / g), which is beneficial to the mass transfer process, thus showing high moisture absorption capacity and is expected to play a role in the fields of atmospheric water collection, soil improvement and humidity monitoring.

[0028] (4) The preparation process of the porous hygroscopic gel of the present invention is simple, economical and practical, does not require special equipment and harsh conditions, has practical value, and is easy to mass produce. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0030] Figure 1 is the infrared spectrum of the ternary deep eutectic solvent prepared in Examples 1 to 4;

[0031] Figure 2 Differential scanning calorimetry (DSC) of the ternary deep eutectic solvents prepared in Examples 1 to 4;

[0032] Figure 3 This is a contact angle photograph of the ternary deep eutectic solvent prepared in Example 3 on the surface of soy protein isolate;

[0033] Figure 4 a~f are optical microscope photos of high internal phase emulsions prepared in Examples 1-5 and 7, respectively;

[0034] Figure 5 The scanning electron microscope (SEM) images of the gels prepared in Example 3 and Comparative Example 1, a is Example 3, b is Comparative Example 1;

[0035] Figure 6 Mercury intrusion test curves of the gels prepared in Example 3 and Comparative Example 1;

[0036] Figure 7 The pore size distribution curves of the gels prepared in Example 3 and Comparative Example 1;

[0037] Figure 8 The water absorption performance of the gel prepared in Example 3 and Comparative Example 1 under different humidity environments; a is 100% humidity, b is 75% humidity;

[0038] Fig. 9 The Raman spectra of a low eutectic solvent and b gel in Example 3; c surface and d cross-section in situ Raman mapping of the gel;

[0039] Fig.10 The moisture absorption (Figure a) and water retention (Figure b) of the improved soil and real soil in Experimental Example 1. DETAILED DESCRIPTION

[0040] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0041] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0042] A first typical embodiment of the present invention provides a porous absorbent gel composition comprising the following components:

[0043] A ternary polymerizable deep eutectic solvent, composed of a monomer, a hydrogen bond acceptor and a hydrogen bond donor;

[0044] Stabilizers;

[0045] internal phase;

[0046] Initiator;

[0047] Cross-linking agent;

[0048] Accelerator.

[0049] In one or more embodiments, the hydrogen bond acceptor comprises choline chloride.

[0050] In one or more embodiments, the hydrogen bond donor includes urea, ethylene glycol or glycerol, preferably urea.

[0051] In one or more embodiments, the monomer includes acrylamide, acrylic acid or methacrylic acid, preferably acrylamide. In the present invention, the monomer acts as a hydrogen bond donor, and combines with another hydrogen bond donor and a hydrogen bond acceptor to form a ternary polymerizable low eutectic solvent. The ternary low eutectic solvent provided in the present invention has both polymerizability and hygroscopicity, and can form a gel in situ without the addition of an external polymerizable monomer; the hygroscopicity of the original polymerizable low eutectic solvent is improved, and the defect of the original low eutectic solvent polymer lacking flexibility is overcome, thereby providing a new idea for the selection of hygroscopic gel dispersion medium.

[0052] In one or more embodiments, the molar ratio of the monomer, the hydrogen bond acceptor and the hydrogen bond donor is 0.5 to 2:1:2.

[0053] In one or more embodiments, the internal phase includes n-hexane.

[0054] In one or more embodiments, the volume ratio of the internal phase in the high internal phase emulsion is greater than 74%, preferably 75%.

[0055] In one or more embodiments, the stabilizer is an amphiphilic polymer, including soy protein isolate. The content of soy protein isolate is 10 to 40 mg / mL. In order to ensure that the emulsion does not break during the polymerization process and maintain a complete template structure, a stabilizer needs to be added during the preparation of a high internal phase emulsion. If the stabilizer content is too low, a stable high internal phase emulsion cannot be obtained, and demulsification is likely to occur during the polymerization process, thereby losing the template effect of the emulsion. If the stabilizer content is too high, the excess stabilizer will dissolve in the external phase low eutectic solvent, causing the external phase viscosity to be too high, which is not conducive to the formation of a high internal phase emulsion.

[0056] In one or more embodiments, the initiator includes ammonium persulfate; the cross-linking agent includes N,N'-methylenebisacrylamide, and the accelerator includes N,N,N',N'-tetramethylethylenediamine.

[0057] A second typical embodiment of the present invention provides a porous absorbent gel, wherein the porous absorbent gel composition is used to form a high internal phase emulsion gel, and the internal phase is removed to form a porous structure with high porosity.

[0058] A third typical embodiment of the present invention provides a method for preparing the porous hygroscopic gel, comprising the following steps:

[0059] (1) mixing a monomer, a hydrogen bond acceptor, and a hydrogen bond donor and heating them to form a ternary polymerizable low eutectic solvent;

[0060] (2) adding a stabilizer and an internal phase to the ternary polymerizable low eutectic solvent in (1), and obtaining a high internal phase emulsion after homogenization;

[0061] (3) continuing to add initiator, crosslinker and accelerator to the high internal phase emulsion in (2), homogenously mixing to form a template prepolymer solution, initiating external phase polymerization, and obtaining a high internal phase emulsion gel;

[0062] (4) Removing the internal phase from the high internal phase emulsion gel, a porous hygroscopic gel is obtained.

[0063] In one or more embodiments, in step (1), the heating temperature is 75 to 85° C., preferably 80° C.; the heating time is 1.5 to 3 h, preferably 2 h.

[0064] In one or more embodiments, in step (2), the homogenization rate is 1800-2500 rpm, preferably 2000 rpm, and the homogenization time is 4-8 min, preferably 5 min.

[0065] In one or more embodiments, in step (3), when the mixture is homogenized and mixed uniformly, the homogenization rate is 1800 to 2500 rpm, preferably 2000 rpm, and the homogenization time is 1 to 4 min, preferably 2 min.

[0066] In one or more embodiments, in step (3), the external phase polymerization is initiated by thermal initiation at a temperature of 65 to 80° C., preferably 70° C., and the reaction time is 0.5 to 2 h, preferably 1 h.

[0067] In one or more embodiments, in step (4), the internal phase in the high internal phase emulsion gel is removed by heating at a temperature of 50 to 60° C., preferably 55° C., and a heating time of 10 to 15 hours, preferably 12 hours. Under this environment, the internal phase n-hexane will evaporate from the inside of the gel, and during the volatilization process, the n-hexane will break through the droplet barrier to form a highly interpenetrating pore structure.

[0068] A fourth typical embodiment of the present invention provides the use of the porous hygroscopic gel as a self-hygroscopic material in atmospheric water collection.

[0069] A fifth typical embodiment of the present invention provides the use of the porous hygroscopic gel as a self-hygroscopic material in humidity monitoring.

[0070] A sixth typical embodiment of the present invention provides use of the porous hygroscopic gel as a self-hygroscopic material in soil improvement.

[0071] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.

[0072] In the following examples, soy protein isolate (SPI) was purchased from Shanghai MacLean Biochemical Technology Co., Ltd. with a CAS number of 9010-10-0.

[0073] Example 1

[0074] (1) Synthesis of a ternary polymerizable low eutectic solvent: 7 g of choline chloride (ChCl), 6 g of urea (urea), and 1.8 g of acrylamide (AM) were weighed into a round-bottom flask, placed in an 80°C oil bath, and heated for 2 h under magnetic stirring to obtain a transparent low eutectic solvent with a certain viscosity.

[0075] (2) 200 μL of the above-mentioned low eutectic solvent was mixed with 50 μL of ultrapure water, 20 mg of soy protein isolate, and 750 μL of n-hexane, and the mixture was vortexed at 2000 rpm for 5 min to obtain a high internal phase emulsion with the low eutectic solvent as the external phase.

[0076] (3) To the prepared high internal phase emulsion, 1.2 mg of ammonium persulfate, 0.6 mg of N,N'-methylenebisacrylamide and 2 μL of N,N,N',N'-tetramethylethylenediamine were added, mixed at 2000 rpm for 2 min, and then heated in a 70°C oil bath for 1 h to thermally initiate free radical polymerization of acrylamide to form a high internal phase emulsion gel.

[0077] (4) Finally, the high internal phase emulsion gel was placed in a 55° C. vacuum drying oven and vacuum dried for 12 h to completely evaporate the internal phase n-hexane, thereby forming a porous gel with high porosity.

[0078] Example 2

[0079] (1) Synthesis of a ternary polymerizable low eutectic solvent: 7 g of choline chloride, 6 g of urea, and 3.6 g of acrylamide were weighed into a round-bottom flask, placed in an 80° C. oil bath, and heated for 2 h under magnetic stirring to obtain a transparent low eutectic solvent with a certain viscosity.

[0080] (2) 200 μL of the above-mentioned low eutectic solvent was mixed with 50 μL of ultrapure water, 20 mg of soy protein isolate, and 750 μL of n-hexane, and the mixture was vortexed at 2000 rpm for 5 min to obtain a high internal phase emulsion with the low eutectic solvent as the external phase.

[0081] (3) To the prepared high internal phase emulsion, 1.2 mg of ammonium persulfate, 0.6 mg of N,N'-methylenebisacrylamide and 2 μL of N,N,N',N'-tetramethylethylenediamine were added, mixed at 2000 rpm for 2 min, and then heated in a 70°C oil bath for 1 h to thermally initiate free radical polymerization of acrylamide to form a high internal phase emulsion gel.

[0082] (4) Finally, the high internal phase emulsion gel was placed in a 55° C. vacuum drying oven and vacuum dried for 12 h to completely evaporate the internal phase n-hexane, thereby forming a porous gel with high porosity.

[0083] Example 3

[0084] (1) Synthesis of a ternary polymerizable low eutectic solvent: 7 g of choline chloride, 6 g of urea, and 5.3 g of acrylamide were weighed into a round-bottom flask, placed in an 80° C. oil bath, and heated for 2 h under magnetic stirring to obtain a transparent low eutectic solvent with a certain viscosity.

[0085] (2) 200 μL of the above-mentioned low eutectic solvent was mixed with 50 μL of ultrapure water, 20 mg of soy protein isolate, and 750 μL of n-hexane, and the mixture was vortexed at 2000 rpm for 5 min to obtain a high internal phase emulsion with the low eutectic solvent as the external phase.

[0086] (3) To the prepared high internal phase emulsion, 1.2 mg of ammonium persulfate, 0.6 mg of N,N'-methylenebisacrylamide and 2 μL of N,N,N',N'-tetramethylethylenediamine were added, mixed at 2000 rpm for 2 min, and then heated in a 70°C oil bath for 1 h to thermally initiate free radical polymerization of acrylamide to form a high internal phase emulsion gel.

[0087] (4) Finally, the high internal phase emulsion gel was placed in a 55° C. vacuum drying oven and vacuum dried for 12 h to completely evaporate the internal phase n-hexane, thereby forming a porous gel with high porosity.

[0088] Example 4

[0089] (1) Synthesis of a ternary polymerizable low eutectic solvent: 7 g of choline chloride, 6 g of urea, and 7.1 g of acrylamide were weighed into a round-bottom flask, placed in an 80° C. oil bath, and heated for 2 h under magnetic stirring to obtain a transparent low eutectic solvent with a certain viscosity.

[0090] (2) 200 μL of the above-mentioned low eutectic solvent was mixed with 50 μL of ultrapure water, 20 mg of soy protein isolate, and 750 μL of n-hexane, and the mixture was vortexed at 2000 rpm for 5 min to obtain a high internal phase emulsion with the low eutectic solvent as the external phase.

[0091] (3) To the prepared high internal phase emulsion, 1.2 mg of ammonium persulfate, 0.6 mg of N,N'-methylenebisacrylamide and 2 μL of N,N,N',N'-tetramethylethylenediamine were added, mixed at 2000 rpm for 2 min, and then heated in a 70°C oil bath for 1 h to thermally initiate free radical polymerization of acrylamide to form a high internal phase emulsion gel.

[0092] (4) Finally, the high internal phase emulsion gel was placed in a 55° C. vacuum drying oven and vacuum dried for 12 h to completely evaporate the internal phase n-hexane, thereby forming a porous gel with high porosity.

[0093] Example 5

[0094] (1) Synthesis of a ternary polymerizable low eutectic solvent: 7 g of choline chloride, 6 g of urea, and 5.3 g of acrylamide were weighed into a round-bottom flask, placed in an 80° C. oil bath, and heated for 2 h under magnetic stirring to obtain a transparent low eutectic solvent with a certain viscosity.

[0095] (2) 200 μL of the above-mentioned low eutectic solvent was mixed with 50 μL of ultrapure water, 10 mg of soy protein isolate, and 750 μL of n-hexane, and the mixture was vortexed at 2000 rpm for 5 min to obtain a high internal phase emulsion with the low eutectic solvent as the external phase.

[0096] (3) To the prepared high internal phase emulsion, 1.2 mg of ammonium persulfate, 0.6 mg of N,N'-methylenebisacrylamide and 2 μL of N,N,N',N'-tetramethylethylenediamine were added, mixed at 2000 rpm for 2 min, and then heated in a 70°C oil bath for 1 h to thermally initiate free radical polymerization of acrylamide to form a high internal phase emulsion gel.

[0097] (4) Finally, the high internal phase emulsion gel was placed in a 55° C. vacuum drying oven and vacuum dried for 12 h to completely evaporate the internal phase n-hexane, thereby forming a porous gel with high porosity.

[0098] Example 6

[0099] (1) Synthesis of a ternary polymerizable low eutectic solvent: 7 g of choline chloride, 6 g of urea, and 5.3 g of acrylamide were weighed into a round-bottom flask, placed in an 80° C. oil bath, and heated for 2 h under magnetic stirring to obtain a transparent low eutectic solvent with a certain viscosity.

[0100] (2) 200 μL of the above-mentioned low eutectic solvent was mixed with 50 μL of ultrapure water, 30 mg of soy protein isolate, and 750 μL of n-hexane, and the mixture was vortexed at 2000 rpm for 5 min to obtain a high internal phase emulsion with the low eutectic solvent as the external phase.

[0101] (3) To the prepared high internal phase emulsion, 1.2 mg of ammonium persulfate, 0.6 mg of N,N'-methylenebisacrylamide and 2 μL of N,N,N',N'-tetramethylethylenediamine were added, mixed at 2000 rpm for 2 min, and then heated in a 70°C oil bath for 1 h to thermally initiate free radical polymerization of acrylamide to form a high internal phase emulsion gel.

[0102] (4) Finally, the high internal phase emulsion gel was placed in a 55° C. vacuum drying oven and vacuum dried for 12 h to completely evaporate the internal phase n-hexane, thereby forming a porous gel with high porosity.

[0103] Example 7

[0104] (1) Synthesis of a ternary polymerizable low eutectic solvent: 7 g of choline chloride, 6 g of urea, and 5.3 g of acrylamide were weighed into a round-bottom flask, placed in an 80° C. oil bath, and heated for 2 h under magnetic stirring to obtain a transparent low eutectic solvent with a certain viscosity.

[0105] (2) 200 μL of the above-mentioned low eutectic solvent was mixed with 50 μL of ultrapure water, 40 mg of soy protein isolate, and 750 μL of n-hexane, and the mixture was vortexed at 2000 rpm for 5 min to obtain a high internal phase emulsion with the low eutectic solvent as the external phase.

[0106] (3) To the prepared high internal phase emulsion, 1.2 mg of ammonium persulfate, 0.6 mg of N,N'-methylenebisacrylamide and 2 μL of N,N,N',N'-tetramethylethylenediamine were added, mixed at 2000 rpm for 2 min, and then heated in a 70°C oil bath for 1 h to thermally initiate free radical polymerization of acrylamide to form a high internal phase emulsion gel.

[0107] (4) Finally, the high internal phase emulsion gel was placed in a 55° C. vacuum drying oven and vacuum dried for 12 h to completely evaporate the internal phase n-hexane, thereby forming a porous gel with high porosity.

[0108] Comparative Example 1

[0109] 200 μL of the ternary polymerizable low eutectic solvent prepared in Example 3 was mixed with 20 mg of soy protein isolate, 1.2 mg of ammonium persulfate, 0.6 mg of N,N′-methylenebisacrylamide and 2 μL of N,N,N′,N′-tetramethylethylenediamine at 2000 rpm for 2 min and then heated in an oil bath at 70°C for 1 h to thermally initiate free radical polymerization of acrylamide to form a low eutectic solvent gel without high porosity.

[0110] Comparative Example 2

[0111] (1) Synthesis of a binary polymerizable low eutectic solvent: 7 g of choline chloride and 5.3 g of acrylamide were weighed into a round-bottom flask, placed in an 80° C. oil bath, and heated for 2 h under magnetic stirring to obtain a transparent low eutectic solvent with a certain viscosity.

[0112] (2) 200 μL of the above-mentioned low eutectic solvent was mixed with 50 μL of ultrapure water, 20 mg of soy protein isolate, and 750 μL of n-hexane, and the mixture was vortexed at 2000 rpm for 5 min. However, a stable high internal phase emulsion could not be formed.

[0113] (3) To the unstable emulsion, 1.2 mg of ammonium persulfate, 0.6 mg of N,N'-methylenebisacrylamide and 2 μL of N,N,N',N'-tetramethylethylenediamine were added, mixed at 2000 rpm for 2 min, and then heated in an oil bath at 70 °C to thermally initiate free radical polymerization of acrylamide to form an emulsion gel. During the polymerization process, the emulsion broke and separated, and could not serve as a template to introduce a highly interconnected pore structure into the gel.

[0114] The structure and performance characteristics are as follows:

[0115] (1) Characterization of ternary polymerizable deep eutectic solvents:

[0116] The ternary deep eutectic solvents prepared in Examples 1 to 7 are transparent liquids with a certain viscosity. The successful preparation of the DES is verified by infrared, differential scanning calorimetry (DSC) and contact angle tests.

[0117] Figure 1 is the infrared spectrum of the ternary deep eutectic solvent prepared in Examples 1 to 4, from Figure 1 It can be seen that when acrylamide is added to choline chloride and urea, 3033 cm -1 The characteristic peak of acrylamide appears at 1625 cm -1 CN bond and 1440cm -1 The CH stretching vibration peak at moves toward the lower wavenumber direction due to the formation of more hydrogen bonds, which proves the hydrogen bonding effect between the three.

[0118] Figure 2 The differential scanning calorimetry (DSC) analysis of the ternary deep eutectic solvents prepared in Examples 1 to 4 shows that Figure 2 It can be seen that the melting point of the low eutectic solvent formed by choline chloride and urea is around 12°C. With the addition of acrylamide, the melting point of the low eutectic solvent gradually increases, which further proves the successful preparation of the ternary low eutectic solvent.

[0119] Figure 3 The contact angle photograph of the ternary deep eutectic solvent prepared in Example 3 on the surface of soy protein isolate is shown in FIG. Figure 3 It can be seen that soy protein isolate has a higher affinity for the low eutectic solvent, and the addition of acrylamide further enhances its wettability to soy protein isolate, which is conducive to the formation of a high internal phase emulsion with the low eutectic solvent as the external phase.

[0120] (2) Characterization of high internal phase emulsion template:

[0121] The high internal phase emulsions prepared in Examples 1 to 7 are opaque emulsions and do not flow when inverted. Figure 4 ) It can be observed that the emulsion is composed of a large number of densely packed droplets, showing the typical structural characteristics of a high internal phase emulsion.

[0122] The effect of the deep eutectic solvent composition on the emulsion formation was further investigated. Figure 4 ad), with the low eutectic solvent as the external phase, the emulsion droplets gradually decreased with the increase of acrylamide, which may be related to the changes in its contact angle and interfacial tension.

[0123] Then the effect of stabilizer content on emulsion formation was investigated ( Figure 4 e, c, f), it was found that with the increase of the content of the stabilizer soy protein isolate, the emulsion droplets gradually decreased. This is because with the increase of the stabilizer content, more stabilizers can be adsorbed to the interface to stabilize the emulsion. Therefore, the emulsion structure can be adjusted by adjusting the components of the low eutectic solvent and the content of the stabilizer, so as to prepare emulsion gels with different pore sizes using this as a template to adjust the gel structure.

[0124] If a conventional binary polymerizable low eutectic solvent is used as the external phase, even if the content of the stabilizer is further increased, a stable high internal phase emulsion cannot be formed, and the emulsion will break after standing at room temperature for 3 hours, and complete phase separation will occur. Due to its instability, the emulsion formed in Comparative Example 2 will also undergo complete phase separation during the gel polymerization process, and the emulsion droplets cannot be stably dispersed in the dispersion medium as a template to introduce a porous structure into the gel.

[0125] Finally, a porous gel (Example 3) prepared by using a low eutectic solvent with a molar ratio of choline chloride, urea and acrylamide of 1:2:1.5 and a high internal phase emulsion with a stabilizer content of 20 mg / mL as a template was compared with the original gel (Comparative Example 1). Because at this ratio, a relatively small amount of stabilizer can be used to prepare an emulsion with uniform and stable droplet size, thereby reducing costs.

[0126] (3) Characterization of porous hygroscopic gel (AWHG):

[0127] The porous hygroscopic gels prepared in Examples 1 to 7 are opaque, lightweight porous gels with good viscoelasticity.

[0128] Figure 5 The scanning electron microscope (SEM) images of the gels prepared in Example 3 and Comparative Example 1 show that the porous gel prepared with the emulsion as the template has a highly interconnected porous structure, with a macropore size of about 40 μm, which is formed after the internal phase of the emulsion template evaporates, consistent with the size observed under the emulsion microscope, while the average pore size of the gel without the template is about 3 μm, and there is no highly interpenetrating multi-level pore structure. The small pores on the macropore walls of the AWHG are generated by the volume shrinkage during the polymerization of the monomer. Mercury intrusion test ( Figure 6 and 7 ) also showed that the porosity (59.5%) and specific surface area (37.5 m 2 / g) are significantly higher than those of the gel without template (porosity: 26.3%; specific surface area: 22.9 m 2 This interconnected high porosity is beneficial to the mass transfer process and can improve the atmospheric water collection capacity of the gel.

[0129] (4) Hygroscopicity of gel:

[0130] First, under the condition of 100% humidity, the high porosity of the porous hygroscopic gel makes it more efficient in water absorption, and it can achieve swelling equilibrium within 10 minutes, and its total water absorption is 4 times that of the control sample ( Figure 8 a). The hygroscopicity of the same porous hygroscopic gel at 70% humidity is also higher than that of the control sample ( Figure 8 b) This shows the effectiveness of the porous structure.

[0131] (5) Hygroscopic mechanism of gel:

[0132] From the Raman spectrum ( Fig. 9 In a), it can be seen that the characteristic peak of water molecules, namely the hydroxyl absorption peak, is at 3300 cm -1 At 3300 cm -1 In addition to the hydroxyl absorption peak at 2900cm-1 There is also an absorption peak of a CH bond at the bottom. After polymerizing it to form a porous hygroscopic gel, these two characteristic absorption peaks are still maintained ( Fig. 9 b). Therefore, the ratio of the peak areas of the two can be used to examine the progress of the gel hygroscopic process. Fig. 9 c) and cross section ( Fig. 9 d) From the mapping spectrum, it can be seen that with the extension of time, due to the presence of hydrophilic groups such as hydroxyl and amino groups on the gel surface, water molecules are gradually adsorbed on the gel surface, and due to the existence of osmotic pressure, water molecules gradually penetrate into the gel, thereby realizing the collection of atmospheric water.

[0133] Experimental Example 1

[0134] Soil improvement application: The porous hygroscopic gel of the present invention is mixed with soil, and the moisture absorption and water retention capacity of the gel soil is examined through the mass change.

[0135] Fig.10 a shows that the moisture absorption capacity of the soil modified by the porous hygroscopic gel is 8 times that of the original soil under the condition of room temperature and humidity of 70%. And after one month of environmental storage ( Fig.10 b), its moisture retention capacity is also significantly higher than that of the original soil, which is beneficial to the growth of plants and crops, and is expected to play a role in soil moisture retention and soil improvement.

[0136] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A porous hygroscopic gel composition, characterized in that: Includes the following components: A ternary polymerizable deep eutectic solvent, composed of a monomer, a hydrogen bond acceptor and a hydrogen bond donor; Stabilizers; internal phase; Initiator; Cross-linking agent; Accelerator.

2. The porous absorbent gel composition according to claim 1, wherein The hydrogen bond acceptor includes choline chloride; Or, the hydrogen bond donor comprises urea, ethylene glycol or glycerol, preferably urea; Or, the monomer comprises acrylamide, acrylic acid or methacrylic acid, preferably acrylamide; Or, the molar ratio of the monomer, the hydrogen bond acceptor and the hydrogen bond donor is 0.5 to 2:1:2; Or, the internal phase comprises n-hexane; Or, the volume ratio of the internal phase in the high internal phase emulsion is greater than 74%, preferably 75%; Or, the stabilizer is an amphiphilic polymer, including soy protein isolate, preferably, the content of soy protein isolate is 10-40 mg / mL; Alternatively, the initiator comprises ammonium persulfate; the cross-linking agent comprises N,N'-methylenebisacrylamide, and the accelerator comprises N,N,N',N'-tetramethylethylenediamine.

3. A porous hygroscopic gel, characterized in that: The porous absorbent gel composition of claim 1 is used to form a high internal phase emulsion gel, and the internal phase is removed to form a porous structure with high porosity.

4. The method for preparing the porous hygroscopic gel according to claim 3, characterized in that: The following steps are involved: (1) mixing a monomer, a hydrogen bond acceptor, and a hydrogen bond donor and heating the mixture to form a ternary polymerizable low eutectic solvent; (2) adding a stabilizer and an internal phase to the ternary polymerizable low eutectic solvent in (1), and obtaining a high internal phase emulsion after homogenization; (3) continuing to add initiator, crosslinker and accelerator to the high internal phase emulsion in (2), homogenously mixing to form a template prepolymer solution, initiating external phase polymerization, and obtaining a high internal phase emulsion gel; (4) Removing the internal phase from the high internal phase emulsion gel, a porous hygroscopic gel is obtained.

5. The preparation method according to claim 4, characterized in that: In step (1), the heating temperature is 75 to 85° C., preferably 80° C.; the heating time is 1.5 to 3 h, preferably 2 h; Alternatively, in step (2), the homogenization rate is 1800-2500 rpm, preferably 2000 rpm, and the homogenization time is 4-8 min, preferably 5 min.

6. The preparation method according to claim 4, characterized in that: In step (3), the homogenization rate is 1800-2500 rpm, preferably 2000 rpm, and the homogenization time is 1-4 min, preferably 2 min; Alternatively, in step (3), the external phase polymerization is initiated by thermal initiation, the thermal initiation temperature is 65 to 80° C., preferably 70° C., and the reaction time is 0.5 to 2 h, preferably 1 h.

7. The preparation method according to claim 4, characterized in that: In step (4), the internal phase in the high internal phase emulsion gel is removed by heating, the heating temperature is 50-60° C., preferably 55° C., and the heating time is 10-15 h, preferably 12 h.

8. Use of the porous hygroscopic gel according to claim 3 as a self-hygroscopic material in atmospheric water collection.

9. Use of the porous hygroscopic gel according to claim 3 as a self-hygroscopic material in humidity monitoring.

10. Use of the porous hygroscopic gel according to claim 3 as a self-hygroscopic material in soil improvement.

Citation Information

Patent Citations

  • Method for preparing macroporous quick-response polyacrylamide hydrogel by adopting frontal polymerization of acrylamide deep-eutectic solvent

    CN111040074A

  • Hydroxyethyl acrylate eutectic solvent, poly (hydroxyethyl acrylate) hydrogel, and preparation method and application of poly (hydroxyethyl acrylate) hydrogel

    CN112898480A

  • Porous polymer gel as well as preparation method and application thereof

    CN117024655A

  • Porous polymer based on polymerizable eutectic solvent and preparation method thereof

    CN117801358A

  • Hydrogen bond induced high stability porous covalent organic gel material and preparation method thereof

    US20220251257A1