Polyurethane foam material as well as preparation method and application thereof
By using room temperature non-reactive polyurethane foaming material during battery pack potting, combined with the design of inhibitors and heat-sensitive catalysts, the inconsistency of glue amount and safety problems are solved, and the consistency and high safety of the material are achieved. Lightweight and safety requirements of the battery pack.
Patent Information
- Application Number
- CN202411281925.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-15
AI Technical Summary
The existing polyurethane foam glue is inconsistent during the battery pack potting process due to the fast reaction speed and increased viscosity, which cannot meet the uniformity and safety requirements of all parts in the battery pack.
Using polyurethane foaming material that is almost unreacted at room temperature, the glue liquid leveling time is extended by adding inhibitors and heat-sensitive catalysts to component A, and the curing is accelerated after heating, ensuring that all parts are cured simultaneously and combining polymers. Polyols, foaming agents and flame retardants improve the impact resistance, thermal conductivity and flame retardant properties of the material.
The consistency and structural stability of the materials in the battery pack are achieved, the risk of thermal spread is reduced, the safety is improved, and the lightweight design requirements are met.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_4
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyurethane materials, and in particular relates to a polyurethane foam material and a preparation method and application thereof. Background Art
[0002] In order to achieve higher volume utilization and higher energy density, in terms of battery pack structure, there is a clear trend towards large cells, large modules, module removal and integration. Battery companies and vehicle manufacturers have maximized the volume utilization of battery packs by improving and streamlining the cells, modules, battery packs and other links. In addition, it is also critical to develop lightweight materials to reduce the weight of the entire battery pack and thus increase the energy density of the system, such as using polymer covers to replace traditional metal covers, using potting materials to replace some metal structural parts, and using foaming materials to replace solid potting materials to reduce density, heat insulation and structural fixation.
[0003] In the battery pack potting solution, the use of low-density polyurethane foam to fill the battery pack cavity has been widely used in the industry.
[0004] However, due to the complex and irregular flow channels in the battery compartment of the battery pack, conventional two-component polyurethane foam adhesive will react within 3 to 5 minutes after mixing, and the viscosity will slowly increase, making it impossible to flow in the narrow gap between the battery cells. As a result, in actual working conditions, the battery pack cavity often has inconsistent glue amounts in different places. In addition, the battery cell has a large specific heat capacity and absorbs heat severely during curing, which also leads to inconsistent curing and foaming effects in different parts, and the overall uniformity of the material cannot be guaranteed. For example, at the location where the battery pack side wall has a large amount of glue, the heat storage is large and the curing speed is fast, and the surface can be dried within 30 minutes. However, at the location where the gap between the battery cells has a small amount of glue and a low temperature, it takes 2 to 24 hours for foaming and curing to achieve surface drying. The different curing speeds result in inconsistent pore size and foaming height, and differences in mechanical properties and thermal conductivity, which will ultimately affect the service life of the battery pack.
[0005] Therefore, in view of the above problems, it is necessary to develop a polyurethane foam material that does not react at room temperature and cures when heated. Summary of the invention
[0006] In view of the deficiencies in the prior art, the object of the present invention is to provide a polyurethane foam material and a preparation method and application thereof. The polyurethane foam material hardly reacts at room temperature, and thus has a more ample leveling time as a potting glue. After leveling, it can be heated and quickly cured and formed. After forming, it has low density, excellent impact resistance, low thermal conductivity and excellent flame retardant properties, which meets the design requirements of battery packs for lightweight and high safety.
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a polyurethane foam material, wherein the polyurethane foam material comprises a component A and a component B;
[0009]
[0010] The component B comprises the following components in parts by weight:
[0011] 40-50 parts by weight of isocyanate;
[0012] 1 to 5 parts by weight of antioxidant
[0013] The polyurethane foam material provided by the present invention is a two-component material, specifically comprising a component A and a component B, wherein the component A comprises a specific number of polymer polyols, a foaming agent, a flame retardant, an inhibitor and a thermosensitive catalyst, and the component B comprises an isocyanate;
[0014] On the one hand, the present invention adds an inhibitor and a thermosensitive catalyst to component A so that the glue obtained after the component A and component B are mixed will hardly react at room temperature, and then the glue has sufficient leveling time when poured into the battery pack, and can be filled into various gaps in the battery pack. After the glue is leveled, the entire battery pack is heated to accelerate the curing and forming of the glue, thereby ensuring that the glue in different parts of the battery pack can be cured at the same time, thereby effectively improving the consistency of the materials in various parts, and making the structure of the encapsulated battery pack more reliable;
[0015] On the other hand, the present invention can ensure that the polyurethane foam material obtained after curing has excellent impact resistance, low thermal conductivity, excellent flame retardant performance and low density by selecting polymer polyols and adding flame retardants and foaming agents; specifically, due to its excellent impact resistance, it can absorb external stress and energy generated by impact, strengthen the fixing effect on the battery cell structure, and maintain the structural stability of the entire battery module; due to its low thermal conductivity, in the case of thermal runaway of the battery cell, the polyurethane foam material filled in the gap between the battery cells can effectively inhibit the heat from propagating to adjacent battery cells, thereby reducing the risk of heat spread and improving the safety of the module; at the same time, due to its good flame retardant and fireproof properties, in extreme cases, when the battery cell catches fire, the flame spread speed can be effectively slowed down, giving the crew a longer safe evacuation time, and the lasting flame retardant effect ensures that the material still has a relatively reliable flame retardant effect after long-term operation and aging; in addition, due to its very low density, it can meet the lightweight design requirements of the battery CTP module.
[0016] Wherein, the amount of the polymer polyol can be 40 parts by weight, 42 parts by weight, 44 parts by weight, 46 parts by weight, 48 parts by weight, 50 parts by weight, 52 parts by weight, 54 parts by weight, 56 parts by weight, 58 parts by weight or 60 parts by weight, etc.
[0017] The amount of the foaming agent can be 0.2 parts by weight, 0.3 parts by weight, 0.4 parts by weight, 0.5 parts by weight, 0.6 parts by weight, 0.7 parts by weight, 0.8 parts by weight, 0.9 parts by weight or 1 part by weight, etc.
[0018] The amount of the flame retardant can be 3 parts by weight, 5 parts by weight, 6 parts by weight, 7 parts by weight, 8 parts by weight, 9 parts by weight, 10 parts by weight, 11 parts by weight, 12 parts by weight, 13 parts by weight, 14 parts by weight or 15 parts by weight, etc.
[0019] The inhibitor may be used in an amount of 0.1 parts by weight, 0.2 parts by weight, 0.3 parts by weight, 0.4 parts by weight, or 0.5 parts by weight.
[0020] The amount of the thermosensitive catalyst can be 0.2 parts by weight, 0.3 parts by weight, 0.4 parts by weight, 0.5 parts by weight, 0.6 parts by weight, 0.7 parts by weight, 0.8 parts by weight, 0.9 parts by weight or 1 part by weight, etc.
[0021] The amount of the isocyanate can be 40 parts by weight, 42 parts by weight, 44 parts by weight, 46 parts by weight, 48 parts by weight or 50 parts by weight.
[0022] Preferably, the antioxidant is used in an amount of 1 part by weight, 2 parts by weight, 3 parts by weight, 4 parts by weight or 5 parts by weight.
[0023] Preferably, the polymer polyol includes polyester polyol and / or polyether polyol, and more preferably is a combination of polyester polyol and polyether polyol.
[0024] Preferably, the content of polyester polyol in the polyurethane foam material is 20 to 30 parts by weight, for example, 21 parts by weight, 22 parts by weight, 23 parts by weight, 24 parts by weight, 25 parts by weight, 26 parts by weight, 27 parts by weight, 28 parts by weight, 29 parts by weight or 30 parts by weight.
[0025] Preferably, the viscosity of the polyester polyol is 100 to 10000 cps, for example, 100 cps, 200 cps, 400 cps, 600 cps, 800 cps or 1000 cps.
[0026] Preferably, the hydroxyl value of the polyester polyol is 100-500 mgKOH / g, for example, 100 mgKOH / g, 150 mgKOH / g, 200 mgKOH / g, 250 mgKOH / g, 300 mgKOH / g, 400 mgKOH / g or 500 mgKOH / g.
[0027] Preferably, the polyester polyol includes any one of phthalic anhydride polyester polyol, polycarbonate polyol or polycaprolactone polyol, or a combination of at least two thereof.
[0028] Preferably, the content of polyether polyol in the polyurethane foam material is 20 to 30 parts by weight, for example, 21 parts by weight, 22 parts by weight, 23 parts by weight, 24 parts by weight, 25 parts by weight, 26 parts by weight, 27 parts by weight, 28 parts by weight, 29 parts by weight or 30 parts by weight.
[0029] Preferably, the viscosity of the polyether polyol is 100-15000 cps, for example, 100 cps, 500 cps, 1000 cps, 2000 cps, 3000 cps, 5000 cps, 7000 cps, 9000 cps, 11000 cps, 13000 cps or 15000 cps.
[0030] Preferably, the hydroxyl value of the polyether polyol is 50-600 mgKOH / g, for example, 50 mgKOH / g, 100 mgKOH / g, 150 mgKOH / g, 200 mgKOH / g, 250 mgKOH / g, 300 mgKOH / g, 350 mgKOH / g, 400 mgKOH / g, 450 mgKOH / g, 500 mgKOH / g, 550 mgKOH / g or 600 mgKOH / g, etc.
[0031] Preferably, the polyether polyol includes any one of sucrose polyether polyol, sorbitol polyether polyol, glycerol polyether polyol, toluene diamine polyether polyol, castor oil modified polyether polyol or PTMG polyether polyol, or a combination of at least two thereof.
[0032] Preferably, the blowing agent includes any one of water, cyclopentane or monofluorodichloroethane, or a combination of at least two thereof.
[0033] Preferably, the flame retardant includes a phosphate ester liquid flame retardant and / or a solid flame retardant.
[0034] Preferably, the phosphate ester liquid flame retardant includes any one of triethyl phosphate (TEP), tri(1-chloro-2-propyl) phosphate (TCPP) or isopropylated triphenyl phosphate (IPPP) or a combination of at least two thereof.
[0035] Preferably, the solid flame retardant includes any one of ammonium polyphosphate (APP), triphenyl phosphate (TPP) or melamine phosphate, or a combination of at least two thereof.
[0036] Preferably, the inhibitor comprises a protonic acid organic compound.
[0037] Preferably, the protonic acid organic compound includes any one or a combination of at least two of hydrochloric acid, phosphoric acid or an organic acid containing 2 to 10 (e.g., 2, 3, 4, 5, 6, 7, 8 or 9, etc.) carbon atoms, and is more preferably a carboxylic acid containing 5 to 10 carbon atoms.
[0038] Preferably, the carboxylic acid containing 5 to 10 carbon atoms includes any one of pentanoic acid, hexanoic acid, heptanoic acid, octanoic acid, nonanoic acid or decanoic acid, or a combination of at least two thereof.
[0039] Preferably, the activation temperature of the thermosensitive catalyst is 40-80°C, for example, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C or 80°C.
[0040] Preferably, the thermosensitive catalyst comprises an organic acid salt of 1,8-diazabicyclo[5.4.0]undec-7-ene.
[0041] Preferably, the component A also includes a foam stabilizer.
[0042] Preferably, the content of the foam stabilizer in component A is 3 to 5 parts by weight, for example, 3.2 parts by weight, 3.4 parts by weight, 3.6 parts by weight, 3.8 parts by weight, 4 parts by weight, 4.2 parts by weight, 4.4 parts by weight, 4.6 parts by weight, 4.8 parts by weight or 5 parts by weight.
[0043] Preferably, the foam stabilizer comprises a polyether-modified organic silicon compound.
[0044] Preferably, the isocyanate includes any one or a combination of at least two of polyphenyl polymethylene polyisocyanate (PAPI), diphenylmethane diisocyanate (MDI) or toluene diisocyanate (TDI).
[0045] Preferably, the B component further comprises an antioxidant.
[0046] Preferably, the content of the antioxidant in the component B is 1 to 5 parts by weight, for example, 1 part by weight, 1.5 parts by weight, 2 parts by weight, 2.5 parts by weight, 3 parts by weight, 3.5 parts by weight, 4 parts by weight, 4.5 parts by weight or 5 parts by weight.
[0047] Preferably, the antioxidant comprises hindered phenol compounds and / or phosphite compounds.
[0048] Preferably, the molar ratio of the hydroxyl group in the A component to the isocyanate group in the B component is 1:(1-2), for example, 1:1.1, 1:1.2, 1:1.4, 1:1.6, 1:1.8 or 1:2, etc.
[0049] Preferably, the free cell density of the polyurethane foam material is 0.1 to 0.7 g / cm 3 , for example 0.1 g / cm 3 , 0.2g / cm 3 , 0.3g / cm 3 , 0.4g / cm 3 , 0.5g / cm 3 , 0.6g / cm 3 or 0.7g / cm 3 wait.
[0050] In the present invention, the theoretical glue injection amount needs to be calculated according to the free bubble density and the glue injection volume of the polyurethane foam material, and then 1.2 to 1.5 times of the theoretical glue injection amount is used as the actual glue injection amount.
[0051] In a second aspect, the present invention provides a method for preparing the polyurethane foam material as described in the first aspect, wherein the preparation method comprises the preparation of component A and the preparation of component B;
[0052] The preparation method of the A component comprises: mixing a polymer polyol, a flame retardant, an inhibitor and optionally a foam stabilizer, adding a foaming agent and a thermosensitive catalyst and mixing them to obtain the A component;
[0053] The preparation method of the B component comprises: mixing isocyanate and an antioxidant to obtain the B component.
[0054] Preferably, the preparation method of the A component specifically comprises: mixing a polymer polyol, a flame retardant, an inhibitor and optionally a foam stabilizer at 100 to 150° C. (e.g., 100° C., 110° C., 120° C., 130° C., 140° C. or 150° C., etc.) and -0.8 to -1 MPa (e.g., -0.82 MPa, -0.84 MPa, -0.86 MPa, -0.88 MPa, -0.9 MPa, -0.92 MPa, -0.94 MPa, -0.96 MPa, -0.97 MPa, -0.98 MPa, -0.99 MPa, -0.10 MPa, -0.11 MPa, -0.12 MPa, -0.13 MPa, -0.14 MPa, -0.15 MPa, -0.16 MPa, -0.17 MPa, -0.18 MPa, -0.19 MPa, -10 MPa, -11 MPa, -12 MPa, -13 MPa, -14 MPa, -15 MPa, The mixture is mixed under a vacuum degree of 0.98 MPa or -1 MPa for 2 to 4 h (for example, 2.2 h, 2.4 h, 2.6 h, 2.8 h, 3 h, 3.2 h, 3.4 h, 3.6 h, 3.8 h or 4 h, etc.), cooled to below 40 ° C (for example, 35 ° C, 30 ° C, 25 ° C, 20 ° C, 15 ° C or 10 ° C, etc.), a blowing agent and a thermosensitive catalyst are added and mixed for 0.5 to 1 h (for example, 0.5 h, 0.6 h, 0.7 h, 0.8 h or 0.9 h, etc.) to obtain the A component.
[0055] Preferably, the preparation method of the B component specifically comprises: mixing the isocyanate and the antioxidant at 30-45°C (for example, 30°C, 35°C, 40°C or 45°C, etc.) and a vacuum degree of -0.8 to -1MPa (for example, -0.82MPa, -0.84MPa, -0.86MPa, -0.88MPa, -0.9MPa, -0.92MPa, -0.94MPa, -0.96MPa, -0.98MPa or -1MPa, etc.) for 0.5-1.5h (for example, 0.5h, 0.7h, 0.9h, 1.1h, 1.3h or 1.5h, etc.) to obtain the B component.
[0056] In a third aspect, the present invention provides a potted battery pack, the potted battery pack comprising a battery pack and a potting glue disposed inside the battery pack;
[0057] The potting glue is obtained by curing the polyurethane foam material as described in the first aspect.
[0058] In a fourth aspect, the present invention provides a method for preparing the encapsulated battery pack according to the third aspect, the preparation method comprising the following steps:
[0059] (1) mixing component A and component B of the polyurethane foam material described in the first aspect to obtain a glue solution;
[0060] (2) The glue obtained in step (1) is poured into the battery pack and cured to obtain the encapsulated battery pack.
[0061] Preferably, the mixing temperature in step (1) is 20-35°C, for example, 20°C, 22°C, 24°C, 26°C, 28°C, 30°C, 32°C, 34°C or 35°C.
[0062] Preferably, the mixing in step (1) is carried out under stirring conditions at a rotation speed of 2000 to 4000 rpm (eg, 2000 rpm, 2500 rpm, 3000 rpm, 3500 rpm or 4000 rpm, etc.).
[0063] Preferably, the mixing time in step (1) is 3 to 5 minutes, for example, 3 minutes, 3.5 minutes, 4 minutes, 4.5 minutes or 5 minutes.
[0064] Preferably, step (2) further includes a standing step before the curing and molding. The standing process allows the potting glue to be fully leveled in the battery pack, and then the cover and pressure-maintaining tooling can be locked, and then the whole is heated and cured.
[0065] Preferably, the standing time is 10 to 30 min, for example, 10 min, 12 min, 14 min, 16 min, 18 min, 20 min, 22 min, 24 min, 26 min, 28 min or 30 min.
[0066] Preferably, the curing temperature in step (2) is 40-80°C, for example, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C or 80°C.
[0067] Preferably, the curing time in step (2) is 0.5 to 2 h, for example, 0.7 h, 0.9 h, 1.1 h, 1.2 h, 1.4 h, 1.6 h, 1.8 h or 2 h.
[0068] Compared with the prior art, the present invention has the following beneficial effects:
[0069] (1) The polyurethane foam material provided by the present invention hardly reacts at room temperature, and thus has sufficient leveling time when poured into the battery pack as a potting glue, and can be filled into various gaps in the battery pack. After leveling, the whole body can be formed by heating and curing, thereby ensuring the consistency of materials in various parts, making the structure of the obtained potted battery pack more reliable;
[0070] (2) The polyurethane foam material provided by the present invention has a certain strength after being formed, and can absorb the stress generated by the outside and the energy generated by the impact, thereby strengthening the fixing effect on the battery cell structure and maintaining the structural stability of the entire battery pack;
[0071] (3) The polyurethane foam material provided by the present invention has a low thermal conductivity after molding. When a battery cell has thermal runaway, the foam material filled in the gap between the battery cells can effectively inhibit the heat from spreading to adjacent battery cells, thereby reducing the risk of heat spread and improving the safety of the battery pack.
[0072] (4) The polyurethane foam material provided by the present invention also has good flame retardant and fireproof properties after molding. In extreme cases, when the battery cell catches fire, it can effectively slow down the spread of the flame, giving the crew members a longer safe evacuation time. At the same time, the long-lasting flame retardant effect can also ensure that the material still has a relatively reliable flame retardant effect after long-term operation and aging;
[0073] (5) The polyurethane foam material provided by the present invention has a very low density and can meet the design requirements of lightweight battery CTP modules. DETAILED DESCRIPTION
[0074] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0075] Some of the raw material information involved in the following specific implementation is as follows:
[0076] (A1) Polyester polyol
[0077] Phthalic anhydride polyester polyol: viscosity 700cps / 25℃, hydroxyl value 320mgKOH / g, purchased from China Ruinuo Chemical, brand PS-3152;
[0078] Polycarbonate polyol: viscosity 500cps / 75℃, hydroxyl value 110mgKOH / g, purchased from Ube Chemical, China, brand PH-100;
[0079] Polycaprolactone polyol: viscosity is 9000 cps / 25°C, hydroxyl value is 56 mgKOH / g, purchased from Daicel Chemical Co., Ltd., China, brand name PCL 220AL.
[0080] (A2) Polyether polyol
[0081] Sucrose polyether polyol: viscosity 2500cps / 25℃, hydroxyl value 450mgKOH / g, purchased from Hebei Yadong Chemical Industry, China, brand name YD-450;
[0082] Toluene diamine polyether polyol: viscosity 13000cps / 25℃, hydroxyl value 400mgKOH / g, purchased from Hebei Yadong Chemical Industry, China, brand name YD-401P;
[0083] PTMG polyether polyol: viscosity is 1200cps / 40°C, hydroxyl value is 56mgKOH / g, purchased from Dalian, Taiwan, China, brand name is PTG2000.
[0084] (A3) Blowing agent: water, cyclopentane or monofluorodichloroethane, all of which are commercially available.
[0085] (A4) Flame retardant: specifically TCPP, purchased from China Wansheng Chemical Group, brand name WSFR-TCPP.
[0086] (A5) Inhibitor: valeric acid, hydrochloric acid, phosphoric acid or acetic acid, all of which are commercially available.
[0087] (A6) Thermosensitive catalyst: specifically, an organic acid salt of 1,8-diazabicyclo[5.4.0]undec-7-ene, with an activation temperature of 60° C., purchased from Guangzhou Yourun Chemical Industry, China, with a brand name of RM-60.
[0088] (A7) Foam stabilizer: polyether modified silicone compound, purchased from Momentive, Germany, brand number L-580.
[0089] (B1) Isocyanate
[0090] PAPI: polyphenyl polymethylene polyisocyanate, commonly available in the market;
[0091] MDI: polyphenyl polymethylene polyisocyanate, commonly available in the market;
[0092] TDI: Toluene diisocyanate, commonly available in the market.
[0093] (B2) Antioxidants
[0094] Antioxidant 1010: hindered phenolic compound, commonly available in the market;
[0095] Antioxidant 168: phosphite compound, commonly available in the market.
[0096] Examples 1 to 8
[0097] Embodiments 1 to 8 provide a polyurethane foam material, each comprising a component A and a component B, wherein the molar ratio of the hydroxyl group (-OH) in the component A to the isocyanate group (-NCO) in the component B is 1:1.5;
[0098] The specific components and amounts of component A are shown in Table 1-1, and the specific components and amounts of component B are shown in Table 1-2. In Tables 1-1 and 1-2, the units of the amounts of each component are "parts by weight".
[0099] Table 1-1
[0100]
[0101] The preparation method of the component A comprises: weighing polyether polyol, polyester polyol, flame retardant, inhibitor and foam stabilizer, stirring and mixing at 120° C. and vacuum degree of -1 MPa for 3 hours, cooling to below 40° C., adding foaming agent and thermosensitive catalyst, continuing to mix at vacuum degree of -1 MPa for 1 hour, discharging, sealing and storing, and obtaining the component A;
[0102] Table 1-2
[0103]
[0104]
[0105] The preparation method of the B component comprises: mixing isocyanate and antioxidant at 40° C. and a vacuum degree of −1 MPa for 1 hour, discharging the mixture, and sealing and storing the mixture to obtain the B component.
[0106] Comparative Examples 1 to 7
[0107] Comparative Examples 1 to 7 respectively provide a polyurethane foam material, each comprising a component A and a component B, wherein the molar ratio of the hydroxyl group (-OH) in the component A to the isocyanate group (-NCO) in the component B is 1:1.5;
[0108] The specific components and amounts of component A are shown in Table 2-1, and the specific components and amounts of component B are shown in Table 2-2. In Tables 2-1 and 2-2, the units of the amounts of each component are "parts by weight".
[0109] Table 2-1
[0110]
[0111] The preparation method of the component A comprises: weighing polyether polyol, polyester polyol, flame retardant, inhibitor and foam stabilizer, stirring and mixing at 120° C. and vacuum degree of -1 MPa for 3 hours, cooling to below 40° C., adding foaming agent and thermosensitive catalyst, continuing to mix at vacuum degree of -1 MPa for 1 hour, discharging, sealing and storing, and obtaining the component A;
[0112] Table 2-2
[0113]
[0114]
[0115] The preparation method of the B component comprises: mixing isocyanate and antioxidant at 40° C. and a vacuum degree of −1 MPa for 1 hour, discharging the mixture, and sealing and storing the mixture to obtain the B component.
[0116] Application Examples 1 to 8 and Comparative Application Examples 1 to 7
[0117] Application Examples 1 to 8 and Comparative Application Examples 1 to 7 respectively provide a potted battery pack, and the preparation method thereof includes the following steps:
[0118] (1) Component A and component B of the polyurethane foam material provided in Examples 1 to 7 were mixed at 30° C. and a stirring speed of 3000 rpm for 4 min to obtain a potting glue;
[0119] (2) The potting glue made of the polyurethane foam material provided in Examples 1 to 7 was poured into the battery pack using a high-pressure foaming machine. After completion, the battery pack was left to stand for 20 minutes. The upper cover and the pressure-maintaining tool were locked and placed in an infrared oven. The battery pack was baked at 60° C. for 1 hour to obtain the potted battery pack.
[0120] Performance Test:
[0121] (1) The initial viscosity of the potting compound at room temperature and the viscosity after standing for 10 minutes at room temperature: refer to the standard GB / T 2794-2022 Determination of adhesive viscosity;
[0122] (2) Compression strength: Refer to GBT 8813-2008 Determination of compression properties of rigid foam plastics;
[0123] (3) Flame retardancy: Determination of flame retardancy according to the reference standard GB-T 8333-2022 Test method for combustion performance of rigid foam plastics;
[0124] (4) Thermal conductivity: Refer to the standard GBT 10294-2008 Determination of steady-state thermal resistance of insulation materials - Determination by the protective plate method;
[0125] (5) Density: Determination according to GB / T6343-2009 “Determination of apparent density of foam plastics and rubber”.
[0126] The polyurethane foam materials provided in Examples 1 to 8 and Comparative Examples 1 to 7 were tested according to the above test method. The test results are shown in Table 3:
[0127] Table 3
[0128]
[0129] From the data in Table 3, we can see that:
[0130] The polyurethane foam materials provided in Examples 1 to 8 have a low viscosity increase after standing for 10 minutes at room temperature, a compressive strength of 2.32 to 2.67 MPa after curing, a flame retardant property of V0 level, a thermal conductivity of 0.031 to 0.038 W / m·K, and a density of only 0.225 to 0.253 g / cm 2 , with low density, excellent flame retardancy, impact resistance and low thermal conductivity.
[0131] Compared with Example 1, the polyurethane foam materials provided in Comparative Examples 1-2 have too low an inhibitor added or even no inhibitor added, resulting in a rapid increase in viscosity after standing at room temperature, and insufficient leveling time after being poured into the battery pack.
[0132] Compared with Example 1, the polyurethane foam material provided in Comparative Example 3 has a low compression strength after curing and does not have excellent impact resistance due to excessive addition of inhibitors.
[0133] Compared with Example 1, the amount of the thermosensitive catalyst added in the polyurethane foam material provided in Comparative Example 4 is relatively low, which also results in low compressive strength after curing and molding, and lacks excellent impact resistance.
[0134] Compared with Example 1, the amount of the thermosensitive catalyst added to the polyurethane foam material provided in Comparative Example 5 is too high, and Comparative Example 6 uses a conventional dibutyltin dilaurate catalyst, both of which result in a rapid increase in viscosity after standing at room temperature, and the flow does not have sufficient leveling time after being poured into the battery pack.
[0135] Compared with Example 1, no flame retardant is added to the polyurethane foam material provided in Comparative Example 7, resulting in a flame retardant grade of only HB after curing and molding, and poor flame retardancy.
[0136] The applicant declares that the present invention illustrates a polyurethane foam material and its preparation method and application through the above embodiments, but the present invention is not limited to the above embodiments, that is, it does not mean that the present invention must rely on the above embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A polyurethane foam material, characterized in that: The polyurethane foam material comprises component A and component B; The A component comprises the following components in parts by weight: The component B comprises the following components in parts by weight: 40-50 parts by weight of isocyanate; 1 to 5 parts by weight of antioxidant 2. The polyurethane foam material according to claim 1, characterized in that: The polymer polyol comprises polyester polyol and / or polyether polyol, preferably a combination of polyester polyol and polyether polyol; Preferably, the content of polyester polyol in the polyurethane foam material is 20 to 30 parts by weight; Preferably, the viscosity of the polyester polyol is 100 to 10000 cps; Preferably, the hydroxyl value of the polyester polyol is 50 to 500 mgKOH / g; Preferably, the polyester polyol comprises any one or a combination of at least two of phthalic anhydride polyester polyol, polycarbonate polyol or polycaprolactone polyol; Preferably, the content of polyether polyol in the polyurethane foam material is 20 to 30 parts by weight; Preferably, the viscosity of the polyether polyol is 100 to 15000 cps; Preferably, the hydroxyl value of the polyether polyol is 50 to 600 mgKOH / g; Preferably, the polyether polyol includes any one of sucrose polyether polyol, sorbitol polyether polyol, glycerol polyether polyol, toluene diamine polyether polyol, castor oil modified polyether polyol or PTMG polyether polyol, or a combination of at least two thereof.
3. The polyurethane foam material according to claim 1 or 2, characterized in that: The foaming agent includes any one of water, cyclopentane or monofluorodichloroethane or a combination of at least two thereof; Preferably, the flame retardant comprises a phosphate ester liquid flame retardant and / or a solid flame retardant; Preferably, the phosphate ester liquid flame retardant includes any one of triethyl phosphate, tri(1-chloro-2-propyl) phosphate or isopropylated triphenyl phosphate or a combination of at least two thereof; Preferably, the solid flame retardant comprises any one or a combination of at least two of ammonium polyphosphate, triphenyl phosphate or melamine phosphate; Preferably, the inhibitor comprises a protonic acid organic compound; Preferably, the protonic acid organic compound includes any one of hydrochloric acid, phosphoric acid or an organic acid containing 2 to 10 carbon atoms or a combination of at least two thereof, and more preferably a carboxylic acid containing 5 to 10 carbon atoms; Preferably, the carboxylic acid containing 5 to 10 carbon atoms includes any one of pentanoic acid, hexanoic acid, heptanoic acid, octanoic acid, nonanoic acid or decanoic acid, or a combination of at least two thereof; Preferably, the activation temperature of the thermosensitive catalyst is 40 to 80°C; Preferably, the thermosensitive catalyst comprises an organic acid salt of 1,8-diazabicyclo[5.4.0]undec-7-ene.
4. The polyurethane foam material according to any one of claims 1 to 3, characterized in that: The A component also includes a foam stabilizer; Preferably, the content of the foam stabilizer in the component A is 3 to 5 parts by weight; Preferably, the foam stabilizer comprises a polyether-modified organic silicon compound.
5. The polyurethane foam material according to any one of claims 1 to 4, characterized in that: The isocyanate includes any one or a combination of at least two of polyphenyl polymethylene polyisocyanate, diphenylmethane diisocyanate or toluene diisocyanate; Preferably, the antioxidant comprises hindered phenol compounds and / or phosphite compounds.
6. The polyurethane foam material according to any one of claims 1 to 5, characterized in that: The molar ratio of the hydroxyl group in the A component to the isocyanate group in the B component is 1:(1-2); Preferably, the free cell density of the polyurethane foam material is 0.1 to 0.7 g / cm 3 .
7. A method for preparing the polyurethane foam material according to any one of claims 1 to 6, characterized in that: The preparation method includes the preparation of component A and the preparation of component B; The preparation method of the A component comprises: mixing a polymer polyol, a flame retardant, an inhibitor and optionally a foam stabilizer, adding a foaming agent and a thermosensitive catalyst and mixing them to obtain the A component; The preparation method of the B component comprises: mixing isocyanate and an antioxidant to obtain the B component.
8. The preparation method according to claim 7, characterized in that: The preparation method of the A component specifically comprises: mixing a polymer polyol, a flame retardant, an inhibitor and an optional foam stabilizer at 100 to 150° C. and a vacuum degree of -0.8 to -1 MPa for 2 to 4 hours, cooling to below 40° C., adding a foaming agent and a thermosensitive catalyst and continuing to mix for 0.5 to 1 hour to obtain the A component; Preferably, the preparation method of the B component specifically comprises: mixing the isocyanate and the antioxidant at 30 to 45° C. and a vacuum degree of -0.8 to -1 MPa for 0.5 to 1.5 h to obtain the B component.
9. A potted battery pack, characterized in that: The potted battery pack includes a battery pack and a potting glue arranged inside the battery pack; The potting glue is obtained by curing the polyurethane foam material according to any one of claims 1 to 6.
10. A method for preparing a potted battery pack as claimed in claim 9, characterized in that: The preparation method comprises the following steps: (1) Mixing component A and component B of the polyurethane foam material according to any one of claims 1 to 6 to obtain a glue solution; (2) pouring the glue obtained in step (1) into the battery pack and curing it to obtain the encapsulated battery pack; Preferably, the mixing temperature in step (1) is 20 to 35°C; Preferably, the mixing in step (1) is carried out under stirring conditions at a rotation speed of 2000 to 4000 rpm; Preferably, the mixing time in step (1) is 3 to 5 minutes; Preferably, step (2) further comprises a step of standing still before the curing molding; Preferably, the standing time is 10 to 30 minutes; Preferably, the curing temperature in step (2) is 40 to 80° C. and the curing time is 0.5 to 2 h.
Citation Information
Cited By
Polyurethane thermal insulation material for geothermal well oil pipe and preparation method of polyurethane thermal insulation material
CN119529227A
Polyurethane foam pouring sealant for battery unit and preparation method of polyurethane foam pouring sealant
CN120192739A
Formaldehyde-free vegetable gum and preparation method thereof
CN120484759A
A non-formaldehyde plant gum and a method for preparing the same
CN120484759B