Method for selectively recovering valuable metal from lithium-containing manganese slag and application

By using homo-ion replacement technology and step-by-step roasting method in lithium-containing manganese slag, the problem of poor selectivity of the existing roasting method is solved, efficient recovery of lithium and manganese is achieved, and subsequent processes are simplified and recovery rate is improved.

CN118957279AActive Publication Date: 2024-11-15ANHUI UNIVERSITY OF TECHNOLOGY
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411027857.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

The existing roasting method has poor selectivity when recovering valuable metals, which leads to difficulty in separation of lithium and manganese and a lot of impurities dissolution, affecting the efficiency of subsequent purification and purification processes.

Method used

By adding metal cationic salts with the same valence state and similar ion radius to the lithium-containing manganese slag, using homo-ion replacement technology, calcination and water-impregnation treatment are carried out in steps to achieve selective recovery of lithium and manganese. The specific steps include one-stage calcination and two-stage calcination to form soluble lithium and manganese salts respectively, and optimize the separation of lithium and manganese by controlling the calcination environment atmosphere and salt type.

Benefits of technology

It realizes efficient step-by-step separation and recovery of lithium and manganese, reduces the dissolution of impurities, simplifies the subsequent purification and purification process, improves the recovery rate of lithium and manganese, and avoids the problems of equipment corrosion and filtration difficulties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957279A_ABST
    Figure CN118957279A_ABST
Patent Text Reader

Abstract

The invention discloses a method for selectively recovering valuable metal from lithium-containing manganese slag and application, and belongs to the technical field of resource recycling. The method comprises the steps that the lithium-containing manganese slag is sequentially subjected to the procedures of smelting, first-stage roasting, lithium extraction, second-stage roasting and manganese extraction, selective recovery of lithium and manganese is achieved, monovalent salt is added in the first-stage roasting procedure, divalent salt is added in the second-stage roasting procedure, the volume ratio of oxygen is controlled to be lower than 20% in the first-stage roasting procedure and the second-stage roasting procedure, and the volume ratio of manganese is controlled to be lower than 20% in the second-stage roasting procedure. A lithium-containing solution and a manganese-containing solution are respectively obtained in the lithium extraction process and the manganese extraction process in a water leaching manner. The method can be applied to selective recovery of valuable metals in lithium ion batteries. According to the method, lithium and manganese can be dissolved out step by step, meanwhile, the problems that more impurities are dissolved out, silica gel is easy to form and difficult to filter and the like can be solved, and the subsequent purification process of lithium is shortened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of resource recovery and utilization, and more specifically, relates to a method and application of selectively recovering valuable metals from lithium-manganese slag. Background Art

[0002] Lithium, known as "white oil", is an important basic material for modern industry, especially in the field of new energy, such as lithium batteries. With the continuous growth of global demand for renewable energy and electric vehicles, the demand for lithium batteries has also increased, which has directly promoted the prosperity of the lithium market. In addition, lithium is also widely used in glass, ceramics, aerospace and other fields, further broadening its market prospects. Manganese metal is also of great importance. Manganese is an indispensable alloying element in steel production, which can improve the toughness, wear resistance and corrosion resistance of steel. With the continuous development of global infrastructure construction and real estate industry, the demand for steel will continue to grow, thereby driving the demand for manganese metal. In addition, manganese is also widely used in batteries, magnetic materials and other fields. Especially in emerging battery technologies, manganese, as an important positive electrode material, is also in increasing demand.

[0003] Lithium-ion batteries are widely used in electric vehicles, communications, electronic equipment and other fields because of their long cycle life, large capacity and light weight. With the rapid increase in the use of lithium-ion batteries, it is expected that waste lithium-ion batteries will reach a peak of scrapping by 2025. Waste lithium-ion batteries contain toxic electrolytes and organic diaphragms, which will cause irreversible damage to soil and water quality. In addition, they contain a large amount of strategic key metals Li (2-3%), Mn (2-20%), Co (5-30%), Ni (0.02-10%), and Cu (7-17%). If they are not recycled, it will cause a huge waste of resources.

[0004] The main recycling methods for waste lithium-ion batteries include pyrometallurgy and hydrometallurgy. The pyrometallurgical recycling process has strong adaptability to raw materials and a large processing scale, and is the most promising short-process processing method. However, the difficulty of the current pyrometallurgical process is that the lithium content in conventional smelting slag is not high, and the lithium-containing mineral phase is complex, which makes it difficult to selectively and efficiently extract lithium. In the existing battery slag lithium extraction process, acids such as sulfuric acid and hydrochloric acid are mostly used for roasting.

[0005] After searching, the patent application document with Chinese patent application number 202211074571.0 and application publication date January 31, 2023 discloses a method for selectively separating and recovering lithium and manganese from waste lithium manganate batteries. The method comprises: (1) discharging, disassembling and classifying waste lithium manganate batteries to obtain positive electrode materials, and then subjecting them to high temperature treatment to remove the binder; (2) roasting the lithium manganate positive electrode powder obtained by pretreatment with sulfates such as ferrous sulfate, ferrous sulfate, ammonium sulfate, and ammonium hydrogen sulfate at a certain temperature in two stages to convert the lithium element of lithium manganate into the corresponding sulfate; (3) leaching the roasting product obtained in the second step with water to obtain a lithium sulfate leachate and a leach residue rich in iron and manganese oxides. However, this process is for processing the lithium manganate positive electrode powder obtained after disassembly, the process is complicated and the manganese element is insoluble. It is necessary to further process the filter residue of Fe2O3, Mn2O3 or FeMnO3 to recover manganese.

[0006] The Chinese patent application document with the number of 201610320979.X and the application publication date of May 16, 2016 discloses a method for extracting lithium and manganese from lithium-containing manganese-rich slag. The method is as follows: lithium-containing manganese-rich slag (a product obtained by pyrometallurgy of waste lithium-ion batteries) is slurried with sulfuric acid solution to obtain a mixed slurry; the mixed slurry is kept warm at a temperature not lower than 50°C; the product after the insulation treatment is roasted, the roasting temperature is controlled to be not lower than 150°C, and the roasting time is not less than 30 minutes; the roasted product is leached, and then the solid-liquid separation is performed to obtain a solution containing manganese sulfate and lithium sulfate. However, in the roasting process, aluminum and silicon will be dissolved to varying degrees, making filtration difficult, and the poor selectivity will lead to a complicated subsequent separation process of lithium, manganese and aluminum, and will cause varying degrees of corrosion to the equipment; at the same time, the obtained leaching solution contains both manganese and lithium, and manganese and lithium are not extracted separately.

[0007] Therefore, developing a green and efficient recovery process for valuable elements in lithium-manganese slag will not only help solve the problem of environmental pollution, but also ease the global energy metal resource tension. Summary of the invention

[0008] 1. Problem to be solved

[0009] In view of the problem that the existing roasting method has poor selectivity in recovering valuable metals, the present invention provides a method for selectively recovering valuable metals from lithium-manganese slag, which can achieve step-by-step dissolution of lithium and manganese by optimizing the roasting process. At the same time, it can also solve the problems of excessive dissolution of impurities, easy formation of silica gel, and difficulty in filtering, and shorten the subsequent purification process of lithium.

[0010] 2. Technical solution

[0011] In order to solve the above problems, the technical solution adopted by the present invention is as follows:

[0012] Based on the phenomenon of isomorphism in natural minerals, the present invention adds metal cation salts with the same valence and similar ionic radius to the lithium-manganese slag, and realizes the step-by-step separation and recovery of lithium and manganese through common ion replacement. The details are as follows:

[0013] A method for selectively recovering valuable metals from lithium-manganese slag, comprising the following steps:

[0014] S1. Melting process:

[0015] Smelting the lithium-manganese-containing slag to obtain lithium-manganese-containing smelting slag;

[0016] S2, first stage roasting process:

[0017] The smelting slag in step S1 is mixed with a monovalent salt and then roasted, wherein the volume proportion of oxygen in the roasting environment atmosphere is controlled to be less than 20%, to obtain a roasting product including a soluble lithium salt, an insoluble aluminum silicate and an insoluble manganese silicate;

[0018] S3, lithium extraction process:

[0019] The calcined product obtained in step S2 is water-soaked, and the filtrate obtained by filtration is a lithium-containing solution, and the filter residue is a manganese-rich slag, and the main phases of the manganese-rich slag are aluminum silicate and manganese silicate; wherein the content of divalent Mn (II) in the manganese-rich slag is 3-25%, and the content of tetravalent Mn (IV) is 0.5-2.0%;

[0020] S4, two-stage roasting process:

[0021] The manganese-rich slag in step S3 is dried and mixed with a divalent salt and then roasted, wherein the volume proportion of oxygen in the roasting environment atmosphere is controlled to be less than 20%, and a roasting product is obtained, including a soluble manganese salt and an insoluble aluminosilicate; it should be noted that the oxygen content in the first-stage roasting determines the tetravalent manganese content in the manganese-rich slag, and although the oxygen content in the second-stage roasting does not determine the tetravalent manganese content in the manganese-rich slag, it affects the leaching rate of the second-stage manganese, because too high an oxygen content in the second-stage roasting process will increase the tetravalent manganese content in the second-stage roasting product, thereby affecting the final manganese leaching rate.

[0022] S5, Manganese Extraction Process:

[0023] The roasted product obtained in step S4 is soaked in water, and the filtrate obtained by filtration is a manganese-containing solution, and the filter residue is aluminosilicate. The manganese-containing solution contains divalent manganese, and the filter residue contains a small amount of tetravalent manganese.

[0024] Furthermore, in step S1, the lithium-manganese-containing smelting slag includes but is not limited to lithium-manganese-containing slag obtained by high-temperature reduction smelting of one or more waste lithium-ion batteries (such as lithium manganate batteries, ternary power batteries, etc.) by pyrometallurgical method, wherein the Li content is 0.5-7.5wt%, the mass fraction ratio of Al2O3 to SiO2 is (0.2-3.5):1, and the Mn content is 3-25wt%.

[0025] Furthermore, in step S1, in the smelting process, the smelting conditions are: temperature 1400-1700°C, time ≥20min, and the amount of slag-forming agent SiO2 added in the smelting process satisfies the mass fraction ratio of Al2O3 to SiO2 of (0.25-3.0):1.

[0026] Furthermore, in step S1, the lithium-manganese smelting slag is smelted according to the relevant requirements of YS / T 509.1-2008 (YS / T509.1-2008 Chemical analysis method of spodumene and lepidolite concentrate - Determination of lithium oxide, sodium oxide and potassium oxide content - Flame atomic absorption spectrometry).

[0027] Furthermore, the monovalent salt used in step S2 can be exchanged with monovalent lithium ions, and the monovalent cations are Na + , K + NH4 + ; including one or more of Na2SO4, K2SO4, (NH4)2SO4, KCl, NaCl, NH4Cl, preferably at least one of Na2SO4 and K2SO4, because the melting point of chloride salts is usually lower than that of sulfate salts, and molten salts are formed and separated from the slag during the roasting process, which is not conducive to the reaction kinetics; and in the presence of a weak water vapor atmosphere, chloride salts are easily decomposed into monovalent metal oxides and form a stable silicate phase with the SiO2 component in the lithium-rich manganese slag, and cannot achieve common ion replacement with lithium. Finally, it cannot be ignored that chloride salts are prone to produce hydrogen chloride gas.

[0028] Furthermore, in step S2, the mass ratio of smelting slag to monovalent salt is controlled to be (1-6):1. Within this range, the recovery rate of lithium increases with the increase of monovalent salt, but too much monovalent salt will increase the cost and increase the Na and K contents of the leachate, which is not conducive to subsequent lithium extraction.

[0029] Furthermore, the method for controlling the oxygen content in steps S2 and S4 is: adjusting the oxygen volume fraction in the atmosphere by controlling the flow ratio of the introduced air and the inert gas.

[0030] Furthermore, the calcination temperature in step S2 is 600-1000° C., preferably 700-900° C. The calcination temperature not only affects the reaction intensity of the common ion replacement, but also affects the stability of the calcined product: if the temperature is too low, the material will not react fully; if the temperature is too high, the salt may decompose and is not conducive to improving the recovery rate of lithium.

[0031] Furthermore, the calcination time in step S2 is 0.5 to 3 hours, preferably 1.5 to 2 hours.

[0032] Furthermore, in step S4, the divalent salt can be exchanged with the divalent manganese ion, and the divalent metal cations are Ca 2+ Mg 2+ ; Including anhydrous CaSO4, MgSO4, CaCl2, MgCl2, and / or one or more of CaSO4, MgSO4, CaCl2, MgCl2 containing water of crystallization. The aqueous salt will increase the atmospheric water vapor during the roasting process, promote the decomposition of the chloride salt, and form a small amount of HCl gas, which will corrode the equipment on the one hand and reduce the conversion efficiency of the salt on the other hand. At least one of anhydrous CaCl2 and anhydrous MgCl2 is preferred.

[0033] Furthermore, in step S4, the mass ratio of manganese-rich slag to divalent salt is controlled to be (1-5):1. Within this range, the recovery rate of manganese increases with the increase of divalent salt, but too much divalent salt will increase the cost and increase the calcium and magnesium content of the leachate, increase the viscosity of the leachate, and is not conducive to the subsequent leaching of manganese.

[0034] Furthermore, in step S4, the calcination temperature is 700-1100° C., preferably 800-1000° C., and the calcination time is 0.5-3 h, preferably 1.5-2 h.

[0035] Furthermore, the conditions for water leaching in steps S3 and S5 are: temperature of 10-80°C, leaching time of 2min-2h, liquid-to-solid ratio of (3-50):1mL / g. Preferably, 40-60°C, 10-30min, (10-20):1. Among them, the leaching rate of lithium is greater than 99%, the impurity content in the lithium-containing solution is extremely low, and the concentrations of Ni, Co, Mn, Al, and Si are all lower than 5mg / L; the leaching rate of manganese is greater than 90%, and the impurity metal content in the manganese-containing solution is extremely low, and the concentrations of Ni, Co, Li, Al, and Si are all lower than 5mg / L.

[0036] An application of the above method in recycling lithium-ion batteries, wherein the lithium-manganese slag includes but is not limited to one or more waste lithium-ion batteries.

[0037] In one possible embodiment of the present invention, the present invention relates to a process for extracting lithium and manganese from lithium-containing slag in the pyrometallurgical recovery process of waste lithium-ion batteries, using pyrometallurgical smelting slag of waste lithium batteries as raw materials, using K, Na, NH4 + The filter residue is subjected to a second-stage roasting with one or more salts containing Ca and Mg to obtain a Mn-containing solution with a low impurity content.

[0038] 3. Beneficial effects

[0039] Compared with the prior art, the present invention has the following beneficial effects:

[0040] The present invention adopts a two-step salt roasting process of lithium-manganese-containing slag, which can be used to treat lithium-containing slag after pyrometallurgical smelting of waste lithium-ion batteries. The present invention has the following characteristics:

[0041] (1) Raw material characteristics

[0042] The raw material of the present invention can be lithium-containing slag obtained by high-temperature reduction smelting of waste lithium-ion batteries (such as lithium cobalt oxide batteries, lithium manganese oxide batteries, ternary power batteries, etc.). Compared with natural lithium-containing ores, the raw material of the present invention can be lithium-containing slag obtained by high-temperature smelting of waste lithium-ion batteries (such as lithium cobalt oxide batteries, lithium manganese oxide batteries, ternary power batteries, etc.). Compared with natural lithium-containing ores, the raw material of the present invention can achieve self-transformation of lithium-containing mineral phase after high-temperature smelting, high activity, simple physical phase, and lower impurity ions.

[0043] (2) One-stage calcination has strong selectivity for Li and high Li yield

[0044] The S2-S3 process is an in-situ ion replacement process, which utilizes the isomorphous substitution properties of metal cation salts with the same valence and similar ionic radius and the large difference in chemical potential gradient. The monovalent cations in the salt open up ion channels in the lithium-rich manganese slag, and selectively replace Li under the appropriate conditions of time, temperature, and salt content to form soluble Li salts and insoluble potassium-sodium silicates, thereby achieving mineral phase reconstruction. The salt used in the first-stage roasting does not react with manganese and aluminum, and the concentrated Ni, Co, Mn, Al, and Si in the Li-containing solution are obtained. The concentration is lower than 5ppm. Since the temperature of the salt roasting process is relatively low, no chlorine or sulfur-containing gas will be volatilized, so it will not corrode the equipment. At the same time, the filtering performance is excellent. The leaching rates of manganese, aluminum and silicon are all lower than 1%. There will be no problems such as the difficulty of liquid-solid separation caused by silica gel. The type of salt used is simple. Only one or more of potassium, sodium and ammonium salts are used in the roasting process. The potassium-sodium salt obtained from the lithium precipitation mother liquor obtained in the subsequent preparation of lithium carbonate can be recycled after evaporation and crystallization. At the same time, the recovery rate is higher than that of natural lithium-containing ore, and the recovery rate of lithium is close to 100%;

[0045] (3) The second stage roasting has strong selectivity for Mn and high manganese yield

[0046] The manganese content in lithium-manganese slag is 3-25%. Conventional methods for extracting manganese are mostly sulfuric acid roasting-water leaching, but there is a problem of poor selectivity, resulting in the presence of a large amount of impurity elements such as aluminum and silicon in the manganese-containing solution, and subsequent cumbersome impurity removal procedures are still required. The key to the two-stage manganese extraction of the present invention is the use of a divalent salt roasting method, which can extract manganese with high selectivity. Therefore, the concentrations of Ni, Co, Li, Al, and Si in the Mn-containing solution are all lower than 5ppm; at the same time, controlling the oxygen content in the roasting process to reduce the formation of tetravalent manganese is also the key to improving the manganese recovery rate, because high-valent (>2-valent) manganese is more stable in nature and difficult to achieve ion replacement. Specifically:

[0047] The present application is similar to the principle of S2-S3 in the process of S4-S5, and utilizes the isomorphous substitution property of metal cation salts with the same valence state and similar ionic radius and the property of large difference in chemical potential gradient. The divalent metal cation opens up ion channels, and selectively replaces Mn under the appropriate conditions of time, temperature and salt amount to form soluble manganese salts and insoluble calcium magnesium aluminum silicate, which can not only ensure the integrity of the original lattice structure, but also realize the reconstruction of the mineral phase, and the salt used for the second stage roasting does not react with aluminum; the concentrations of Ni, Co, Li, Al and Si in the obtained Mn-containing solution are all lower than 5ppm, and because the salt roasting process is at a low temperature, no chlorine or sulfur-containing gas volatilization will be generated, so it will not cause corrosion to the equipment, and the leaching rates of aluminum and silicon are both lower than 1%, the filtration performance is excellent, and the problems of difficult liquid-solid separation caused by silica gel will not occur. And the type of salt used is simple, and only one or two calcium salts or magnesium salts are used in the roasting process. The calcium and magnesium waste liquid generated by the subsequent preparation of manganese sulfate or other manganese products can be recycled after evaporation and crystallization to obtain calcium and magnesium salts. At the same time, the recovery rate is higher than that of natural lithium-containing ore, and the recovery rate of Mn is close to 90%.

[0048] (3) The obtained Li-containing solution and Mn-containing solution are widely used in subsequent applications

[0049] The impurity ion content in the Li-containing solution is low. After simple impurity removal, concentration and crystallization, high-purity Li2CO3 can be produced by introducing CO2 or adding potassium and sodium carbonate. The impurity ion content in the Mn-containing solution is low. The pH is adjusted to allow Ca and Mg ions to form precipitation. High-valent manganese can be obtained through concentration, crystallization and low-temperature calcination, which can be used in the production of positive electrode materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] Figure 1 is a process flow chart of the present invention;

[0051] Figure 2 This is a SEM image of the lithium-manganese-containing smelting slag in the embodiment;

[0052] Figure 3 This is the SEM image of the first stage calcined product in Example 1;

[0053] Figure 4 This is the SEM image of the second-stage calcination product in Example 1. DETAILED DESCRIPTION

[0054] The present invention is further described below in conjunction with specific embodiments.

[0055] In order to better understand the present invention, the present invention is further described below through specific implementation methods, but the exemplified embodiments do not limit the protection scope of the present invention.

[0056] In a specific embodiment, the lithium-manganese slag is taken as an example of waste lithium-ion batteries, and valuable metals, lithium and manganese, are recovered from the waste lithium-ion batteries. The specific steps are as follows:

[0057] S1. Melting process:

[0058] The waste lithium-ion batteries were smelted by high-temperature reduction pyrometallurgy to obtain lithium-manganese smelting slag. The smelting conditions were as follows: temperature 1400-1700℃, time ≥20min, and the amount of slag-making agent SiO2 added during the smelting process satisfied the mass fraction ratio of Al2O3 to SiO2 (0.25-3.0):1. The main components of the lithium-manganese smelting slag are shown in Table 1, and the SEM characterization results are shown in Table 1. Figure 2 shown.

[0059] S2, first stage roasting process:

[0060] According to Table 2, the lithium-manganese smelting slag in step S1 is mixed with a monovalent salt and then roasted. The roasting temperature is controlled to be 800° C., the roasting time is 1.5 h, and the oxygen volume fraction in the roasting environment atmosphere is controlled to obtain a roasted product. The SEM characterization results of the roasted product in Example 1 are as follows: Figure 3 As shown, its main phases are soluble lithium salts, insoluble aluminum silicates and insoluble manganese silicates;

[0061] S3, lithium extraction process:

[0062] The roasted product obtained in step S2 is water-leached, and the leaching time of the water-leaching process is 2h, the liquid-to-solid ratio is 20:1mL / g, and the leaching temperature is 60°C; the filtrate obtained by filtration is a lithium-containing solution, and the filter residue is a manganese-rich slag, and the main phases of the manganese-rich slag are aluminum silicate and manganese silicate; wherein the impurity content in the lithium-containing solution is extremely low, and the concentrations of Ni, Co, Mn, Al, and Si are all lower than 5mg / L; the content of divalent Mn (II) in the manganese-rich slag is 3-25%, and the content of tetravalent Mn (IV) is 0.5-2.0%;

[0063] S4, two-stage roasting process:

[0064] According to Table 3, the manganese-rich slag in step S3 is dried and mixed with a divalent salt and then roasted, and the roasting temperature is controlled to be 900°C and the roasting time is 2h; the volume ratio of oxygen in the roasting environment atmosphere is controlled to obtain a roasting product, such as the SEM characterization results of the second-stage roasting product of Example 1. Figure 4 As shown, its main phases include soluble manganese salts and insoluble aluminosilicates;

[0065] S5, Manganese Extraction Process:

[0066] The roasted product obtained in step S4 is water-leached, the leaching time is 1.5 h, the liquid-to-solid ratio is 20:1 mL / g, the leaching temperature is 50° C. The filtrate obtained by filtration is a manganese-containing solution, and the filter residue is aluminosilicate. The impurity metal content in the manganese-containing solution is extremely low, and the concentrations of Ni, Co, Li, Al, and Si are all lower than 5 mg / L.

[0067] Table 1 Detection results of main components of lithium-manganese slag (wt%)

[0068]

[0069] Table 2 Parameters of the first stage roasting process and the content of low-valent manganese in the manganese-rich slag in each embodiment

[0070]

[0071] Table 3 Parameters of the second stage roasting process of each embodiment

[0072]

[0073] It is worth noting that the reaction conditions in the above embodiments are all the optimal reaction conditions for the reaction, and the reaction conditions within the scope of the claims can synthesize the complex of the present invention. In order to avoid redundancy, no examples are given here, such as the temperature and time of the first and second stage roasting. Those skilled in the art can obtain better roasting effects by extending the roasting time at a low roasting temperature within the scope defined by the claims of the present application; in addition, those skilled in the art can reproduce the present invention according to the general formula of the complex of the present invention and the listed related solvents, catalysts and other reagents. Since there are too many examples, several representative examples are selected here, which are sufficient to prove that the complex of the present invention has excellent luminescence efficiency and low oxygen quenching rate, so the examples are not repeated here.

Claims

1. A method for selectively recovering valuable metals from lithium-manganese slag, Features: The lithium-manganese slag is subjected to smelting, first-stage roasting, lithium extraction, second-stage roasting, and manganese extraction processes in sequence to achieve selective recovery of lithium and manganese, wherein a monovalent salt is added in the first-stage roasting process, and a divalent salt is added in the second-stage roasting process, and the volume proportion of oxygen in the first-stage roasting process and the second-stage roasting process is controlled to be less than 20%, and water immersion is adopted in the lithium extraction process and the manganese extraction process to obtain a lithium-containing solution and a manganese-containing solution, respectively.

2. A method for selectively recovering valuable metals from lithium-manganese slag according to claim 1, Features: In the smelting process, the smelting conditions are: temperature 1400-1700°C, time ≥20min.

3. A method for selectively recovering valuable metals from lithium-manganese slag according to claim 1, Features: In the first roasting process, the monovalent salt includes sulfate and / or chloride, wherein the cation of the monovalent salt includes Na + , K + NH 4 + ; Control the mass ratio of smelting slag to monovalent salt to (1~6):

1.

4. A method for selectively recovering valuable metals from lithium-manganese slag according to claim 1, Features: In the second stage roasting process, the divalent salt includes sulfate and / or chloride, wherein the cation of the divalent salt includes Ca 2+ Mg 2+ .

5. A method for selectively recovering valuable metals from lithium-manganese slag according to claim 4, Features: The divalent salt is a salt without crystal water, a salt containing crystal water, or a mixture of a salt without crystal water and a salt containing crystal water; the mass ratio of the manganese-rich slag to the divalent salt is controlled to be (1-5):

1.

6. A method for selectively recovering valuable metals from lithium-manganese slag according to claim 1, Features: In the first stage of the calcination process: the calcination temperature is 600-1000°C, preferably 700-900°C; the calcination time is 0.5-3h, preferably 1.5-2h; In the second-stage calcination process, the calcination temperature is 700-1100° C., preferably 800-1000° C., and the calcination time is 0.5-3 h, preferably 1.5-2 h.

7. A method for selectively recovering valuable metals from lithium-manganese slag according to claim 1, Features: The lithium extraction process is as follows: the calcination product in the first calcination process is leached in water to obtain a filtrate which is a lithium-containing solution, and a filter residue which is a manganese-rich slag, wherein the lithium leaching rate is greater than 99%, and the concentrations of Ni, Co, Mn, Al, and Si in the lithium-containing solution are all lower than 5 mg / L, and the content of Mn(II) in the manganese-rich slag is 3-25%, and the content of Mn(IV) is 0.5-2.0%.

8. A method for selectively recovering valuable metals from lithium-manganese slag according to claim 1, Features: The manganese extraction process is as follows: the calcined product in the second-stage calcination process is leached in water to obtain a filtrate which is a manganese-containing solution, and the filter residue is aluminosilicate, wherein the manganese leaching rate is greater than 90%, and the concentrations of Ni, Co, Li, Al, and Si in the manganese-containing solution are all lower than 5 mg / L.

9. A method for selectively recovering valuable metals from lithium-manganese slag according to any one of claims 1 to 8, Features: The conditions for water immersion are: temperature of 10-80°C, leaching time of 2min-2h, liquid-to-solid ratio of (3-50):1mL / g; preferably 40-60°C, 10-30min, (10-20):

1.

10. Use of the method according to any one of claims 1 to 9 in recycling lithium-ion batteries, Features: The lithium-manganese slag includes but is not limited to one or more waste lithium-ion batteries.

Citation Information

Patent Citations

  • Method for producing manganese sulfate and silver through leaching manganese and silver from manganese-silver ore

    CN106119565A

  • Method for selectively extracting valuable metals from waste lithium ion battery powder based on reduced sodium roasting phase conversion

    CN111254276A

  • Resourceful treatment method for manganese slag and calcium chloride waste residues

    CN113387390A

  • Comprehensive recovery method for valuable components of waste power battery

    CN115074540A

  • Method for selectively separating and recycling lithium and manganese from waste lithium manganate battery

    CN115652077A