Preparation method of thick film printing electrode slurry
By using binders of different molecular weights and specific additives in thick film printing electrode paste, the problems of fast curing speed and poor fluidity caused by high molecular weight adhesives are solved, and the uniform thickness and smooth edges of the slurry are achieved, thereby improving the Printing efficiency and effect.
Patent Information
- Application Number
- CN202411131458.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-18
- Publication Date
- 2024-11-15
AI Technical Summary
When using high molecular weight binder, the existing thick film printing electrode paste has fast curing speed and poor fluidity, resulting in rough printing layer and uneven thickness, which can easily cause dry network and printing defects.
Use binders of different molecular weights (low molecular weight and high molecular weight adhesives) to prepare an organic carrier, and add tributyl citrate, lecithin and hydrogenated castor oil to the printing electrode slurry, and heat it through a constant temperature oil bath pot. Stir to dissolve completely, combine with the powder to ensure the fluidity and thixotropy of the slurry.
Improve the fluidity and thixotropy of the electrode paste, keep the oily and non-drying net, significantly improve the printing efficiency, ensure uniform thickness of the paste after printing, flat edges, avoid edge burrs, and have high viscosity and excellent fluidity. Thixotropy.
Smart Images

Figure CN118969398A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electrostatic chucks, and in particular to a method for preparing thick film printing electrode slurry. Background Art
[0002] The thickness of the electrode slurry used in the electrostatic chuck is required to be between 4 and 20 μm. Thick film printing has higher requirements for the thixotropy, fluidity and curing properties of the electrode slurry. The thixotropy affects the appearance of the printed edge of the slurry, and the fluidity affects the printing of slurry with high fluidity, which is prone to edge bleeding.
[0003] In the prior art, in order to achieve the required thickness of thick film printing paste, it is usually necessary to mix it with an organic carrier with a higher viscosity, that is, a high molecular weight binder is required to increase the viscosity of the organic carrier so as to achieve the required electrode paste thickness. However, the use of high molecular weight binders has the following problems:
[0004] 1. The electrode slurry solidifies quickly, which easily causes dry mesh;
[0005] 2. The fluidity of the electrode slurry is poor, resulting in a rough printed layer and uneven thickness, and may also cause printing defects such as failure to print. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a method for preparing a thick film printed electrode slurry to solve the problem raised in the background technology.
[0007] In order to solve the above technical problems, the technical solution of the present invention is:
[0008] A method for preparing a thick film printed electrode slurry, the preparation method comprising:
[0009] Preparation of organic carrier:
[0010] A solvent is mixed with two or more adhesives, wherein the two or more adhesives have different molecular weights and include at least one low molecular weight adhesive and at least one high molecular weight adhesive, wherein the solvent is 80 wt% terpineol, and 7 wt% tributyl citrate, 1 wt% lecithin, and 2 wt% hydrogenated castor oil are added to the mixture of the solvent and the adhesive;
[0011] First, 80 wt% of terpineol, 7 wt% of tributyl citrate, 1 wt% of lecithin, and 2 wt% of hydrogenated castor oil are mixed, heated and stirred in a constant temperature oil bath, the heating temperature is 50° C. to 80° C., and the stirring speed is 390 to 400 rpm. After mixing, at least one low molecular weight adhesive and at least one high molecular weight adhesive are slowly added to completely dissolve the adhesive, and then stirring is continued for 3 to 6 hours at a stirring speed of 430 to 450 rpm. The prepared organic carrier is canned and cooled at room temperature;
[0012] Preparation of printed electrode slurry:
[0013] The powder is mixed with the above-mentioned organic carrier, and then mixed in a crusher for 40 to 80 minutes to fully blend the two without obvious agglomeration. After the mixing is completed, it is rolled 4 to 6 times in a three-roll mill. The rolled slurry is sieved to remove impurities to obtain a finished slurry, which can be used for subsequent printing tests.
[0014] Preferably, the adhesive is ethyl cellulose or polypropylene resin.
[0015] Preferably, the adhesive is ethyl cellulose EC10 and ethyl cellulose EC100.
[0016] Preferably, when the powder is mixed with the organic carrier, the powder accounts for 75 wt % and the organic carrier accounts for 25 wt %.
[0017] The above technical solution has the following beneficial effects:
[0018] Two or more binders with different molecular weights are used to prepare the organic carrier, so that the electrode slurry can maintain good fluidity and thixotropy while increasing the solid content and viscosity;
[0019] In the thick film printing process, the slurry can keep the oil moist and not dry the net, which can greatly improve the printing efficiency;
[0020] The thickness of the slurry after printing is uniform without saddle shape, and the printed edge is smooth without edge bleeding or burrs. It has high viscosity and excellent fluidity and thixotropy, which is conducive to thick film printing. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a graph showing the change in slurry viscosity with rotation speed in an embodiment of the present invention. DETAILED DESCRIPTION
[0022] The specific embodiments of the present invention are further described below in conjunction with the accompanying drawings. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0023] A method for preparing a thick film printed electrode slurry, the preparation method comprising:
[0024] Preparation of organic carrier:
[0025] A solvent is mixed with two or more adhesives, wherein the two or more adhesives have different molecular weights and include at least one low molecular weight adhesive and at least one high molecular weight adhesive, for example, the adhesives are ethyl cellulose EC10 and ethyl cellulose EC100, wherein the solvent is 80 wt % of pinene alcohol, and 7 wt % of tributyl citrate, 1 wt % of lecithin, and 2 wt % of hydrogenated castor oil are added to the mixture of the solvent and the adhesive;
[0026] First, 80 wt% of terpineol, 7 wt% of tributyl citrate, 1 wt% of lecithin, and 2 wt% of hydrogenated castor oil are mixed, heated and stirred in a constant temperature oil bath, the heating temperature is 50° C. to 80° C., and the stirring speed is 390 to 400 rpm. After mixing, at least one low molecular weight adhesive and at least one high molecular weight adhesive are slowly added to completely dissolve the adhesive, and then stirring is continued for 3 to 6 hours at a stirring speed of 430 to 450 rpm. The prepared organic carrier is canned and cooled at room temperature;
[0027] Preparation of printed electrode slurry:
[0028] The powder is mixed with the above-mentioned organic carrier, wherein the powder is 75wt% and the organic carrier is 25wt%, and then mixed in a crusher for 40-80min to fully blend the two without obvious agglomeration. After the mixing is completed, the three-roll mill is rolled for 4-6 times, and the rolled slurry is sieved to remove impurities to obtain a finished slurry, which can be used for subsequent printing tests;
[0029] Two or more binders with different molecular weights are used to prepare the organic carrier, so that the slurry can maintain good fluidity and thixotropy while increasing the solid content and viscosity; the slurry can remain oily and not dry during thick film printing, greatly improving printing efficiency; the slurry thickness after printing is uniform, without saddle shape, and the printed edge is flat, without edge bleeding and burr problems, so that it has high viscosity and excellent fluidity and thixotropy, which is conducive to thick film printing;
[0030] The basic concept of the method for preparing electrode slurry of the present invention is: using two or more binders in an organic carrier, the key point is that the molecular weight of the added binders is different. If only a low molecular weight binder is used, after the slurry is made, due to the short molecular chain of the binder, it is easy to crack after drying and sintering, and the slurry viscosity is low, and the middle is easy to sink after thick film printing, and the printing effect is poor; if only a high molecular weight binder is used, due to the long molecular chain, the slurry viscosity increases, although the slurry sinking problem will not occur, but the poor fluidity will cause the printing surface to be rough, which will cause uneven printing thickness. The technical solution of the present application adopts binders of different molecular weights to prepare the slurry. On the one hand, it can maintain good thickness uniformity after the slurry is printed, and on the other hand, it can also make the slurry have fluidity and thixotropy.
[0031] Embodiment 1:
[0032] A method for preparing a thick film printed electrode slurry, comprising:
[0033] Preparation of organic carrier:
[0034] Use a precision balance to weigh 80wt% pineol, 7wt% tributyl citrate, 1wt% lecithin, and 2wt% hydrogenated castor oil, mix them in a beaker, place them in an oil bath and heat and stir them, the heating temperature is 60°C, the speed is 400rpm, and 10wt% ethyl cellulose (EC) is weighed again, wherein EC10 accounts for 2.5wt% and EC100 accounts for 7.5wt%, wherein EC10 and EC100 have different molecular weights, one is a low molecular weight adhesive, and the other is a high molecular weight adhesive, slowly add the adhesive into the beaker, after the adhesive is completely melted, increase the speed to 450rpm, continue stirring for 4h, and put the prepared organic carrier into a can and cool it at room temperature;
[0035] Preparation of slurry:
[0036] Weigh 75wt% tungsten powder and 25wt% organic carrier in a mortar, stir and mix them in a pestle for 50 minutes, so that the two are fully integrated without obvious agglomeration; then transfer the slurry mixed by the pestle to a three-roll mill for 4 times, and bottle the slurry for viscosity measurement. Measuring the viscosity change of the slurry at different speeds can reflect its fluidity and thixotropy. The test results are as follows: Figure 1 From the curve 1 in the figure, we can see that as the rotation speed increases, the slurry viscosity decreases. This characteristic is beneficial to improving the slurry printing effect. During the printing process, it has a lower viscosity, a better printing appearance, and a smoother printing surface. At the same time, after the printing stops, the slurry viscosity increases and it is not easy to produce depressions.
[0037] Embodiment 2:
[0038] A method for preparing a thick film printed electrode slurry, comprising:
[0039] Preparation of organic carrier:
[0040] Use a precision balance to weigh 80wt% pineol, 7wt% tributyl citrate, 1wt% lecithin, and 2wt% hydrogenated castor oil, mix them in a beaker, place them in an oil bath and heat and stir them, the heating temperature is 60°C, the speed is 400rpm, and 10wt% ethyl cellulose (EC) is weighed again, wherein EC10 accounts for 7.5wt% and EC100 accounts for 2.5wt%, wherein EC10 and EC100 have different molecular weights, one is a low molecular weight adhesive, and the other is a high molecular weight adhesive, slowly add the adhesive into the beaker, after the adhesive is completely melted, increase the speed to 450rpm, continue stirring for 4h, and put the prepared organic carrier into a can and cool it at room temperature;
[0041] Preparation of slurry:
[0042] Weigh 75wt% tungsten powder and 25wt% organic carrier in a mortar, stir and mix them in a pestle for 50 minutes, so that the two are fully integrated without obvious agglomeration; then transfer the slurry mixed by the pestle to a three-roll mill and roll it for 6 times, and bottle the slurry for viscosity measurement. Measuring the viscosity change of the slurry at different speeds can reflect its fluidity and thixotropy. The test results are as follows: Figure 1 From curve 2 in the figure, it can be seen that, similar to Example 1, as the rotation speed increases, the slurry viscosity decreases, but the degree of viscosity reduction is lower than that of curve 1.
[0043] Comparative Example 1:
[0044] A method for preparing a thick film printed electrode slurry, comprising:
[0045] Preparation of organic carrier:
[0046] Use a precision balance to weigh 80wt% of terpineol, 7wt% of tributyl citrate, 1wt% of lecithin, and 2wt% of hydrogenated castor oil, mix them in a beaker, place them in an oil bath and heat and stir them at 60°C and 400rpm, weigh 10wt% of EC10 again, slowly add the binder into the beaker, increase the speed to 450rpm after the binder is completely melted, continue stirring for 4h, and put the prepared organic carrier into a can and cool it at room temperature;
[0047] Preparation of slurry:
[0048] Weigh 75wt% tungsten powder and 25wt% organic carrier in a mortar, stir and mix them in a pestle for 50 minutes, so that the two are fully integrated without obvious agglomeration; then transfer the slurry mixed by the pestle to a three-roll mill and roll it for 6 times, and bottle the slurry for viscosity measurement. Measuring the viscosity change of the slurry at different speeds can reflect its fluidity and thixotropy. The test results are as follows: Figure 1 From curve 3 in the figure, it can be seen that as the rotor speed increases, the viscosity basically does not change, and the viscosity is relatively thin, so the printing process is prone to problems such as substandard thickness and slurry depression.
[0049] Comparative Example 2:
[0050] A method for preparing a thick film printed electrode slurry, comprising:
[0051] Preparation of organic carrier:
[0052] 80wt% terpineol, 7wt% tributyl citrate, 1wt% lecithin, and 2wt% hydrogenated castor oil were weighed using a precision balance, mixed in a beaker, placed in an oil bath, heated and stirred at 60°C and 400rpm, 10wt% EC100 was weighed again, the binder was slowly added to the beaker, and after the binder was completely melted, the speed was increased to 450rpm, and stirring was continued for 4h, and the prepared organic carrier was canned and cooled at room temperature;
[0053] Preparation of slurry:
[0054] Weigh 75wt% tungsten powder and 25wt% organic carrier in a mortar, stir and mix them in a pestle for 50 minutes, so that the two are fully integrated without obvious agglomeration; then transfer the slurry mixed by the pestle to a three-roll mill and roll it for 6 times, and bottle the slurry for viscosity measurement. Measuring the viscosity change of the slurry at different speeds can reflect its fluidity and thixotropy. The test results are as follows: Figure 1 From curve 4 in FIG. 1 , it can be seen that as the rotor speed increases, the viscosity does not change substantially, and the viscosity is relatively thick, so problems such as uneven printing thickness and poor printing pattern are prone to occur during the printing process.
[0055] The adhesives added in Example 1 and Example 2 include ethyl cellulose EC10 and ethyl cellulose EC100, and the added adhesives have low molecular weight and high molecular weight, while in Comparative Example 1 and Comparative Example 2, only ethyl cellulose EC10 or ethyl cellulose EC100 is added. When only EC10 is added in Comparative Example 1, the printing process is prone to problems such as substandard thickness and slurry depression. In Comparative Example 2, only EC100 is added, and the printing process is prone to problems such as uneven printing thickness and poor printing pattern. The above problems will not occur in Example 1 and Example 2.
[0056] The embodiments of the present invention are described in detail above with reference to the accompanying drawings, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the scope of protection of the present invention.
Claims
1. A method for preparing a thick film printed electrode slurry, characterized in that: The preparation method comprises: Preparation of organic carrier: A solvent is mixed with two or more adhesives, wherein the two or more adhesives have different molecular weights and include at least one low molecular weight adhesive and at least one high molecular weight adhesive, wherein the solvent is 80 wt% terpineol, and 7 wt% tributyl citrate, 1 wt% lecithin, and 2 wt% hydrogenated castor oil are added to the mixture of the solvent and the adhesive; First, 80 wt% of terpineol, 7 wt% of tributyl citrate, 1 wt% of lecithin, and 2 wt% of hydrogenated castor oil are mixed, heated and stirred in a constant temperature oil bath, the heating temperature is 50° C. to 80° C., and the stirring speed is 390 to 400 rpm. After mixing, at least one low molecular weight adhesive and at least one high molecular weight adhesive are slowly added to completely dissolve the adhesive, and then stirring is continued for 3 to 6 hours at a stirring speed of 430 to 450 rpm. The prepared organic carrier is canned and cooled at room temperature; Preparation of printed electrode slurry: The powder is mixed with the above-mentioned organic carrier, and then mixed in a crusher for 40 to 80 minutes to fully blend the two without obvious agglomeration. After the mixing is completed, it is rolled 4 to 6 times in a three-roll mill. The rolled slurry is sieved to remove impurities to obtain a finished slurry, which can be used for subsequent printing tests.
2. The method for preparing a thick film printed electrode slurry according to claim 1, characterized in that: The adhesive is ethyl cellulose and polypropylene resin.
3. The method for preparing a thick film printed electrode slurry according to claim 2, characterized in that: The adhesive is ethyl cellulose EC10 and ethyl cellulose EC100.
4. The method for preparing a thick film printed electrode slurry according to claim 1, characterized in that: When the powder is mixed with the organic carrier, the powder accounts for 75 wt % and the organic carrier accounts for 25 wt %.