Topcon battery and preparation method thereof, photovoltaic module and photovoltaic system

By controlling the thickness and refractive index of the alumina film and anti-reflective film layer, combined with PECVD temperature control, the problem of Topcon battery being sensitive to UV is solved, and an effective UV attenuation effect is achieved, reducing costs and improving the battery's UV resistance ability .

CN118969914APending Publication Date: 2024-11-15RUNMA GUANGNENG TECH (JINHUA) CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411465837.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-21
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing Topcon batteries are sensitive to ultraviolet (UV), resulting in component efficiency and power attenuation. Traditional methods are costly and ineffective, and solutions with improved HJT battery structure cannot be applied to Topcon batteries.

Method used

By controlling the thickness of the alumina film and the composition and refractive index of the first anti-reflective film layer, combined with PECVD temperature control, the alumina layer and the anti-reflective film layer are prepared by ALD and PECVD technologies to improve the UV-induced attenuation effect.

Benefits of technology

It effectively improves the problem of UV-induced attenuation, reduces costs, and avoids the risk of H aggregation on the silicon surface, improves the passivation effect, and enhances the battery's UV resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118969914A_ABST
    Figure CN118969914A_ABST
Patent Text Reader

Abstract

The invention discloses a Topcon battery and a preparation method thereof, a photovoltaic module and a photovoltaic system, and relates to the technical field of photovoltaic cells, and the preparation method of the Topcon battery comprises the steps: 1, providing a substrate which comprises a front surface and a back surface opposite to each other, and carrying out the texturing of the substrate; step 2, carrying out boron diffusion on the substrate; forming a P + layer on the front surface of the substrate; 3, cleaning and polishing the back surface of the substrate, passivating through a silicon dioxide thin film and an amorphous silicon layer, and then performing phosphorus treatment to form an N + layer; 4, the front face is cleaned, and the winding plating of the front face is removed; an aluminum oxide layer with the thickness of 3-6 nm is formed on the P + layer; and 5, respectively depositing a first antireflection film layer and a second antireflection film layer on the front surface and the back surface. By controlling the thickness of the aluminum oxide film and the components and the refractive index of the bottommost antireflection film layer of the first antireflection film layer, the UV-induced degradation can be effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of solar cells, and in particular to Topcon cells and preparation methods thereof, photovoltaic modules, and photovoltaic systems. Background Art

[0002] In recent years, the photovoltaic industry has developed rapidly, technological updates have gradually accelerated, and the photovoltaic industry is moving towards product diversification. Research on Topcon batteries, HJT batteries, BC batteries, and batteries of various technical routes is underway.

[0003] Photovoltaic cells are devices that directly convert light energy into electrical energy through the photoelectric effect or photochemical effect. However, existing cells are sensitive to UV (ultraviolet rays) and are prone to attenuation of module efficiency and power under the action of ultraviolet rays. In traditional technology, the use of light-converting adhesive film to solve the attenuation problem of photovoltaic modules not only leads to increased costs, but also affects the light-conversion effect and life of the adhesive film due to the poor compatibility between the light-converting agent and the adhesive film, resulting in poor results. In addition, there are also related reports on UV improvement for the unique structure of HJT cells, which mainly improves the UV of the doping layer and local contact passivation structure of HJT cells. However, the doping layer and local contact passivation structure are important cell structures of HJT cells. Although their structural optimization can improve UV, it may also cause adverse effects on other performance aspects, or require more structural coordinated processing. In addition, the structure of HJT cells is different from that of Topcon cells. The solution for improving the UV of HJT structure optimization cannot be applied to Topcon cells, and there is no relevant report on the improvement of UV-induced attenuation of Topcon cells. Summary of the invention

[0004] The purpose of the present application is to provide a Topcon cell and a preparation method thereof, a photovoltaic module, and a photovoltaic system. The preparation method of the Topcon cell provided in the present application is simple to operate, low in cost, and can effectively improve the problem of UV-induced attenuation.

[0005] The first aspect of the present application provides a method for preparing a Topcon battery, comprising: Step 1: providing a substrate, wherein the substrate comprises a front side and a back side opposite to each other, and performing a texturing treatment on the substrate; Step 2: performing boron diffusion on the substrate; forming a P+ layer on the front side of the substrate; Step 3: cleaning and polishing the back side of the substrate, passivating it with a silicon dioxide film and an amorphous silicon layer, and then performing phosphorus doping to form an N+ layer; Step 4: Clean the front side of the substrate to remove the front side plating; and form an aluminum oxide layer with a thickness of 3-6 nm on the P+ layer; Step 5: depositing a first anti-reflection film layer and a second anti-reflection film layer on the front side of the substrate and the back side of the substrate respectively; wherein the BC first anti-reflection film layer comprises at least one layer, and the refractive index of the bottom anti-reflection film layer of the first anti-reflection film layer close to the aluminum oxide layer is 2.08-2.30; Step 6: Perform printing and drying treatments on the front side and the back side of the substrate respectively.

[0006] In an optional manner, in step 4, ALD is used to prepare the aluminum oxide layer, wherein water is introduced for 4000-7000 ms at a temperature of 230-300°C, TMA is introduced for 4000-7000 ms after waiting for purge, and then TMA and water are alternately introduced into the cavity and the silicon wafer to react with each other while waiting for purge, and the aluminum oxide layer is obtained after 25-45 cycles of passivation.

[0007] In an optional manner, in step 5, PECVD is used to prepare the first anti-reflection film layer and the second anti-reflection film layer, wherein the operating temperature of PECVD for preparing the first anti-reflection film is greater than the operating temperature of PECVD for preparing the second anti-reflection film.

[0008] In an optional manner, the operating temperature when preparing the first anti-reflection film is 480-540°C; the operating temperature when preparing the second anti-reflection film is 470-520°C.

[0009] In an optional manner, the bottom anti-reflection film layer is a SiNx film, and / or the thickness of the bottom anti-reflection film layer is 10-20 nm.

[0010] Preferably, the method for preparing the bottom anti-reflection film layer is: introducing 6000-12000sccm ammonia, 1000-3000sccm silane, 5000-15000W RF power, 1300mT-2000mT pressure, and 50-200s process time.

[0011] Preferably, the method for preparing the bottom anti-reflection film layer is: introducing silane and ammonia in a ratio of 1:3 to 1:5.

[0012] In an optional manner, the first anti-reflection film layer includes at least two layers, the bottom anti-reflection film layer is a SiNx film, and the other layers are SiNx films, SiONx films or SiOx films.

[0013] Preferably, the sub-bottom anti-reflection film layer arranged on the bottom anti-reflection film layer is a SiNx film, and / or the refractive index of the sub-bottom anti-reflection film layer is 2.15~2.25; and / or the thickness of the sub-bottom anti-reflection film layer is 20~30nm; and / or the method for preparing the sub-bottom anti-reflection film layer is: the ratio of silane and ammonia introduced is 1:5~1:12.

[0014] Preferably, the film arranged on the sub-bottom anti-reflection film layer is a SiONx film; and / or, the refractive index of the SiONx film is 1.7-1.95; and / or, the thickness of the SiONx film layer is 10-40nm; and / or, the method for preparing the SiONx film is: the ratio of introducing silane, ammonia and nitrous oxide is 1: (3-6): (7-10).

[0015] The second aspect of the present application provides a Topcon battery prepared by the Topcon battery preparation method of the first aspect of the present application.

[0016] The third aspect of the present application provides a photovoltaic assembly, comprising the Topcon cell of the second aspect of the present application.

[0017] A fourth aspect of the present application provides a photovoltaic system, comprising the photovoltaic component of the third aspect of the present application.

[0018] Compared with the prior art, this application (1) By controlling the thickness of the aluminum oxide film and the composition and refractive index of the bottom anti-reflection film layer of the first anti-reflection film layer, UV-induced attenuation can be effectively improved.

[0019] (2) By improving the temperature of PECVD, it is avoided to increase the H content at a lower temperature. The binding capacity of H is increased so that a large amount of H is accumulated on the silicon surface. During sintering, H overflows instantly, posing the risk of film explosion. The surface recombination rate of the aluminum oxide film and the aluminum oxide film and the bottom anti-reflection film layer after high-temperature annealing is significantly reduced, which improves UV-induced attenuation and increases the passivation effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings: Figure 1 A schematic flow chart showing the method for preparing the Topcon battery of the present application.

[0021] Figure 2 A schematic diagram showing an embodiment of a Topcon battery of the present application.

[0022] Reference numerals: 1-substrate; 2-P+ layer; 3-aluminum oxide layer; 4-first anti-reflection film layer; 41-bottom anti-reflection film layer; 5-N+ layer; 6-second anti-reflection film layer; 7-front electrode; 8-back electrode. DETAILED DESCRIPTION

[0023] Hereinafter, embodiments of the present disclosure will be described with reference to the accompanying drawings. However, it should be understood that these descriptions are exemplary only and are not intended to limit the scope of the present disclosure. In addition, in the following description, descriptions of well-known structures and technologies are omitted to avoid unnecessary confusion of the concepts of the present disclosure.

[0024] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, "multiple" means two or more, unless otherwise clearly and specifically defined. "Several" means one or more, unless otherwise clearly and specifically defined.

[0025] Photovoltaic cells are sensitive to UV, which can cause the efficiency and power of photovoltaic modules to decay. Therefore, research on how to improve UV attenuation is of great significance to Topcon cells.

[0026] The first aspect of the present application provides a method for preparing a Topcon battery, such as Figure 1 As shown, the following steps are included: Step 1: providing a substrate, the substrate comprising a front side and a back side opposite to each other, and performing a texturing process on the substrate; In this step, the substrate is an N-type single crystal silicon wafer, which includes a relative front and back side. By texturing the N-type single crystal silicon wafer, not only the organic dirt and metal impurities on the surface of the silicon wafer are removed, but also the mechanical damage layer generated in the wire cutting process of the silicon wafer can be removed to reduce the recombination center. The texturing mainly adopts alkaline solution texturing, and the silicon on the surface of the substrate reacts with the alkaline solution to form a pyramid velvet surface on the surface of the silicon wafer.

[0027] In some optional embodiments, the substrate is texturized using sodium hydroxide or potassium hydroxide.

[0028] Step 2: Boron diffusion is performed on the substrate; a P+ layer is formed on the front side of the substrate; In this step, the purpose of boron diffusion is mainly to form a PN junction on the surface of the silicon wafer. It is mainly achieved by vaporizing a boron source (such as BBr3 or BCL3) in a tube furnace and then depositing it on the surface of the silicon wafer through a series of chemical reactions to obtain a suitable doping concentration, junction depth and square resistance; a P+ layer (boron doped layer) is formed on the front side of the silicon wafer; boron diffusion is generally prepared in a low-pressure diffusion furnace, using a boron source and O2 as reaction gases, and N2 as a carrier gas, and reacting at a certain flow rate and temperature.

[0029] In some optional embodiments, BCL3 and O2 are used as reaction gases, N2 is used as carrier gas, the flow rate of BCL3 is 2500sccm, the flow rate of O2 is 500~3000sccm, the flow rate of N2 is 1000~20000sccm, and the doping temperature is 500~900℃.

[0030] Step 3: Clean and polish the back side of the substrate, passivate it with a silicon dioxide film and an amorphous silicon layer, and then dope it with phosphorus to form an N+ layer; In this step, when preparing the N+ layer, it is necessary to first remove the BSG layer (borosilicate glass layer) on the back of the substrate, generally using hydrofluoric acid for removal; then perform alkaline polishing, which mainly uses potassium hydroxide aqueous solution to form a tower base on the surface of the silicon wafer, and deposit a silicon dioxide film and an amorphous silicon layer on the tower base, and then perform phosphorus treatment to obtain the N+ layer.

[0031] The deposition of silicon dioxide film and amorphous silicon layer is prepared by LPCVD. Oxygen is passed through at high temperature under low pressure conditions, and oxygen and silicon react to produce silicon oxide, forming an oxide layer. Silane is then passed through at high temperature, and silane is thermally decomposed into silicon and hydrogen, forming an amorphous silicon layer.

[0032] Through phosphorus diffusion, in the presence of oxygen, POCl3 decomposes at high temperature to generate phosphorus pentachloride (PCl5) and phosphorus pentoxide (P2O5). The generated P2O5 reacts with silicon at the diffusion temperature to generate silicon dioxide (SiO2) and phosphorus atoms, eventually forming an N+ layer.

[0033] Step 4: Clean the front side of the substrate to remove the front side plating; and form an aluminum oxide layer with a thickness of 3-6nm on the P+ layer; In this step, the front and edge PSG layers produced in the previous step are removed, for example, by using hydrofluoric acid and nitric acid; after removal, the aluminum oxide layer is prepared.

[0034] The aluminum oxide layer is mainly deposited by the ALD method, using trimethylaluminum (TMA) as the aluminum source and vaporized water (H2O) or gaseous oxygen (O2) as the oxygen (O) source. Two or more chemical vapor precursors are alternately introduced into the reaction chamber and react on the surface of the substrate to form an aluminum oxide layer.

[0035] The thickness of the aluminum oxide layer is 3-6nm, for example, it can be 3nm, 3.5nm, 4nm, 4.5nm, 5nm, 5.5nm or 6nm; in Topcon cells, as the thickness of the aluminum oxide film increases, the bulk resistivity can be increased, the blocking ability of H atoms can be increased, and the diffusion of H atoms in SiNx into the silicon matrix can be greatly reduced; but if the number of H atoms in the silicon matrix is ​​too low, it is not conducive to resisting potential induced decay; if the number of H atoms in the silicon matrix is ​​too high, it affects UV induced decay. Therefore, the thickness of the aluminum oxide film is generally controlled to select a suitable silicon nitride layer and control its refractive index, so that it has the ability to resist potential induced decay and UV induced decay.

[0036] In some optional embodiments, ALD is used to prepare the aluminum oxide layer at a temperature of 230-300°C, for example, 230°C, 240°C, 250°C, 260°C, 270°C, 280°C, 290°C or 300°C; the time for introducing water is between 4000-7000ms, for example, 4000ms, 5000ms, 6000ms or 7000ms; after waiting for purge, TMA (trimethylaluminum) is introduced for 4000-7000ms, for example, 4000ms, 5000ms, 6000ms or 7000ms; and then waiting for purge is performed, TMA and water alternately enter the cavity, and continuously go through 25-45 cycles, for example, 25 cycles, 26 cycles, 27 cycles, 28 cycles, 29 cycles, 30 cycles, 31 cycles, 32 cycles, 33 cycles, 34 cycles, 35 cycles, 36 cycles, 40 cycles, and 45 cycles.

[0037] Step 5: depositing a first anti-reflection film layer and a second anti-reflection film layer on the front side and the back side of the substrate respectively; wherein the first anti-reflection film layer comprises at least one layer, and the refractive index of the bottom anti-reflection film layer of the first anti-reflection film layer close to the aluminum oxide layer is 2.08-2.30; In this step, the substrate treated with ALD is placed in PECVD to prepare an anti-reflection film layer, a first anti-reflection film layer is formed on the front side of the substrate, and a second anti-reflection film layer is formed on the back side of the substrate; wherein the first anti-reflection film layer includes at least one layer, and the refractive index of the bottom anti-reflection film layer close to the aluminum oxide layer is 2.08~2.30; for example, it can be 2.08, 2.09, 2.10, 2.11, 2.12, 2.13, 2.15, 2.16, 2.17, 2.18, 2.20, 2.22, 2.23, 2.24, 2.25, 2.26, 2.27, 2.28, 2.29 or 2.30.

[0038] Preferably, the refractive index of the bottom anti-reflection film layer is 2.15-2.25.

[0039] The anti-reflection film can be a SiNx film, a SiONx film or a SiOx film; the preparation of the three films is mainly based on the different gases introduced. For example, the SiNx film is prepared by introducing ammonia and silane; the SiONx film is prepared by introducing silane, ammonia and laughing gas; and the SiOx film is prepared by introducing silane and laughing gas.

[0040] In some optional embodiments, PECVD is used to prepare the first anti-reflection film layer and the second anti-reflection film layer, wherein the operating temperature of PECVD for preparing the first anti-reflection film is greater than the operating temperature of PECVD for preparing the second anti-reflection film.

[0041] In some specific embodiments, the operating temperature when preparing the first anti-reflection film is 480-540°C; for example, it can be 480°C, 490°C, 500°C, 510°C, 520°C, 530°C or 540°C. The operating temperature when preparing the second anti-reflection film is 470-520°C; for example, it can be 470°C, 480°C, 490°C, 500°C, 510°C or 520°C. By improving the temperature of PECVD, it is avoided to increase the H content at a lower temperature, increase the binding capacity of H so that a large amount of H is gathered on the silicon surface, and there is a risk of film layer explosion when H overflows instantly during sintering; and the surface recombination rate of the aluminum oxide film and the aluminum oxide film and the bottom anti-reflection film layer after high temperature annealing is significantly reduced, which improves UV-induced attenuation and increases the passivation effect.

[0042] In some optional embodiments, the bottommost anti-reflection film layer of the first anti-reflection film layer is a SiNx film.

[0043] In some optional embodiments, the thickness of the bottom anti-reflection film of the first anti-reflection film layer is 10-20 nm, for example, 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, 15 nm, 16 nm, 17 nm, 18 nm, 19 nm or 20 nm.

[0044] In some optional embodiments, the preparation method of the bottom anti-reflection film layer is as follows: introducing ammonia gas at 6000-12000sccm, for example, 6000sccm, 7000sccm, 8000sccm, 9000sccm, 10000sccm, 11000sccm or 12000sccm; silane at 1000-3000sccm, for example, 1000sccm, 1100sccm, 1200sccm, 1300sccm, 1400sccm, 1500sccm, 1600sccm, 1700sccm, 1800sccm, 1900sccm, 2000sccm, 2500sccm, etc. sccm or 3000sccm; the RF power is 5000-15000W, for example, it can be 5000W, 6000W, 7000W, 8000W, 9000W, 10000W, 11000W, 12000W, 13000W, 14000W or 15000W; the pressure is 1300mT-2000mT, for example, it can be 1300mT, 1400mT, 1500mT, 1600mT, 1700mT, 1800mT, 1900mT or 2000mT; the process time is 50-200s; for example, it can be 50ms, 60ms, 70ms, 80ms, 90ms, 100ms, 110ms, 120ms, 130ms, 140ms, 150 ms, 160 ms, 170 ms, 180 ms, 190 ms or 200 ms.

[0045] In some optional embodiments, the method for preparing the bottom anti-reflection film layer is: the ratio of silane and ammonia introduced is 1:3 to 1:5; for example, it can be 1:3, 1:4, or 1:5.

[0046] In some optional embodiments, the first anti-reflection film layer includes at least two layers, the bottom layer of the first anti-reflection film layer close to the aluminum oxide layer is a SiNx film, and the other layers are at least one of a SiNx film, a SiONx film or a SiOx film; Preferably, starting from the bottom anti-reflection film layer, the first anti-reflection film layer can be SiNx / SiNx / SiNx film; SiNx / SiNx / SiNx / SiONx / SiONx / SiOx film in sequence.

[0047] In some optional embodiments, the sub-bottom anti-reflection film layer arranged in the bottom anti-reflection film layer is a SiNx film, and / or the refractive index is 2.15~2.25; for example, it can be 2.15, 2.16, 2.17, 2.18, 2.19, 2.20, 2.21, 2.22, 2.23, 2.24 or 2.25; and / or the thickness of the sub-bottom anti-reflection film layer is 20~30nm; for example, it can be 20nm, 21nm, 22nm, 23 nm, 24 nm, 25 nm, 26 nm, 27 nm, 28 nm, 29 nm or 30nm.

[0048] In some optional embodiments, the method for preparing the sub-bottom anti-reflection film layer is: the ratio of silane and ammonia gas introduced is 1:5 to 1:12; for example, it can be 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:11 or 1:12; In some optional embodiments, a SiONx film is disposed on the sub-bottom anti-reflection film layer; and / or the refractive index is 1.7-1.95; for example, it may be 1.7, 1.8, 1.9 or 1.95; the thickness of the SiONx film layer is 10-40nm; for example, it may be 10nm, 11nm, 12nm, 13 nm, 14 nm, 15 nm, 16 nm, 17 nm, 18 nm, 19 nm, 20nm, 21nm, 22nm, 23nm, 24 nm, 25 nm, 26 nm, 27 nm, 28 nm, 29 nm, 30nm, 31mm, 32mm, 33mm, 34mm, 35mm, 36mm, 37mm, 38mm, 39mm or 40mm.

[0049] In some optional embodiments, the method for preparing SiONx film is: the ratio of silane, ammonia and nitrous oxide introduced is 1: (3-6): (7-10); for example, it can be 1:3:7, 1:3:8, 1:3:9, 1:3:10, 1:4:7, 1:4:8, 1:4:9, 1:4:10, 1:5:7, 1:5:8, 1:5:9, 1:5:10, 1:6:7, 1:6:8, 1:6:9 or 1:6:10.

[0050] More preferably, the first anti-reflection film layer is a SiNx / SiNx / SiONx film; wherein the bottom anti-reflection film layer is a SiNx film; the refractive index is 2.15~2.25, and the thickness is 10-20nm; the sub-bottom anti-reflection film layer arranged on the bottom anti-reflection film layer is a SiNx film, the refractive index is 2.15~2.25, and the thickness is 20~30nm; a SiONx film is arranged on the sub-bottom anti-reflection film layer; the refractive index is 1.7~1.95; the thickness of the SiONx film layer is 10-40nm.

[0051] Step 6: Print and dry the front and back sides separately.

[0052] In this step, electrodes are prepared on the front and back sides of the substrate. The electrodes are screen-printed, and the main grid and the auxiliary grid are printed on the front and back sides of the substrate. After sintering and light injection, the electrodes are fixed on the surface of the battery to obtain the final product Topcon battery.

[0053] The second aspect of the present application provides a Topcon battery prepared by the Topcon battery preparation method of the first aspect of the present application.

[0054] like Figure 2 As shown, the Topcon cell prepared in the present application includes a substrate 1, the substrate includes a relative front and back side, the front side of the substrate is provided with a P+ layer 2, an aluminum oxide layer 3, a first anti-reflection film layer 4 and a front electrode 7; wherein the first anti-reflection film layer includes a bottom anti-reflection film layer 41 close to the aluminum oxide layer 3; the back side of the substrate is provided with an N+ layer 5, a second anti-reflection film layer 6 and a back electrode 8.

[0055] In some optional embodiments, the UV-induced degradation rate of the Topcon cell after 15kw illumination is less than 0.7%.

[0056] In some optional embodiments, the UV-induced degradation rate of the Topcon cell after 30 kW illumination is less than 1%.

[0057] In some optional embodiments, the UV-induced degradation rate of the Topcon cell after 60 kW illumination is less than 2%.

[0058] The third aspect of the present application provides a photovoltaic assembly, comprising the Topcon cell of the second aspect of the present application.

[0059] A fourth aspect of the present application provides a photovoltaic system, comprising the photovoltaic component of the third aspect of the present application.

[0060] The preparation method of the Topcon battery disclosed in the first aspect of the present application and the Topcon battery disclosed in the second aspect are described in detail below with several specific embodiments. It is worth noting that the following description is only for illustrative purposes and is not a specific limitation of the invention.

[0061] In the following examples, the thickness and refractive index of the anti-reflection film layer are measured by an ellipsometer; the UV-induced attenuation data of the Topcon battery is tested in a UV aging test box, and the battery efficiency data before and after UV irradiation is tested by a battery efficiency tester, and its UV-induced attenuation rate is calculated. Among them, UV-induced attenuation rate % = (efficiency before UV test - efficiency after UV test) / efficiency before UV test.

[0062] Example 1

[0063] An N-type single crystal silicon wafer is selected and textured with sodium hydroxide to form a pyramid texture surface on the surface of the silicon wafer.

[0064] In a low-pressure diffusion furnace, BCL3 and O2 are used as reaction gases, N2 is used as carrier gas, the flow rate of BCL3 is 2500sccm, the flow rate of O2 is 500~3000sccm, the flow rate of N2 is 1000~20000sccm, and the doping temperature is 500~900℃ to prepare the P+ layer. The BSG (borosilicate glass) layer on the back and side surfaces is removed by using a 50% volume fraction hydrofluoric acid solution through a chain pickling device; The back of the substrate is alkaline polished, the temperature of the alkaline tank soaking area is 40-70°C, the concentration is 1%-5%; the alkaline solution is potassium hydroxide aqueous solution; LPCVD is used to deposit silicon dioxide film and amorphous silicon layer. First, at a temperature of 500~700°C, 10000sccm~50000sccm of oxygen is introduced for a deposition time of 1min~30min. Then, at a temperature of 500~600°C, 1000sccm~2000sccm of SiH4 is introduced for a deposition time of 10min~30min.

[0065] When a tubular diffusion furnace is used to prepare phosphorus doping, POCl3 and O2 are used as reaction gases, N2 is used as carrier gas, the flow rate of POCl3 is 2500sccm, the flow rate of O2 is 500~3000sccm, the flow rate of N2 is 1000~20000sccm, and the phosphorus doping temperature is 500~900℃.

[0066] The front and edge PSG layers were removed using hydrofluoric acid and nitric acid.

[0067] The cleaned substrate was placed in the ALD equipment, the operating temperature of the equipment was set to 240°C, water was introduced for 6000ms, TMA was introduced for 6000ms after waiting for purge, and then waiting for purge, alternating the chamber reaction, and after 30 cycles of passivation, an aluminum oxide layer with a thickness of 4.10mm was prepared.

[0068] The substrate treated by ALD is placed in PECVD for preparation of an anti-reflection film layer, wherein a first anti-reflection film layer is formed on the front side of the substrate, and a second anti-reflection film layer is formed on the back side of the substrate.

[0069] The operating temperature for preparing the first anti-reflection film layer on the front side is 520°C, and the operating temperature for preparing the second anti-reflection film layer on the back side is 500°C; The preparation method of the bottom anti-reflection film layer of the first anti-reflection film layer on the front side is as follows: introducing 6000 sccm ammonia and 1500 sccm silane; the RF power supply power is 10000W, the pressure is 1300mT, and the process time is 80s; and a SiNx film is prepared with a film thickness of 15nm and a refractive index of 2.20.

[0070] The main grid and the auxiliary grid are printed on the front and back of the substrate by screen printing, and the electrodes are fixed on the surface of the battery after sintering and light injection to obtain a Topcon battery.

[0071] Example 2

[0072] The difference from Example 1 is: The preparation method of the bottom anti-reflection film layer of the first anti-reflection film layer on the front side is as follows: 7500 sccm of ammonia and 2500 sccm of silane are introduced; the RF power is 10000W, the pressure is 1300mT, and the process time is 80s. The SiNx film is prepared with a film thickness of 20nm and a refractive index of 2.25.

[0073] Example 3

[0074] The difference from Example 1 is: The cleaned substrate was placed in the ALD equipment, the operating temperature of the equipment was set to 240°C, water was introduced for 6000ms, TMA was introduced for 6000ms after waiting for purge, and then waiting for purge, alternating the chamber reaction, and after 35 cycles of passivation, an aluminum oxide layer with a thickness of 4.72mm was prepared.

[0075] The preparation method of the bottom anti-reflection film layer of the first anti-reflection film layer on the front side is as follows: introducing 6000 ammonia and 1500 silane; the RF power is 10000W, the pressure is 1300mT, and the process time is 80s; and a SiNx film is prepared with a film thickness of 20nm and a refractive index of 2.25.

[0076] Then, 9000 ammonia and 1500 silane were introduced, the RF power was 10000 W, the pressure was 1300 mT, and the process time was 80 s; a SiNx film was prepared with a film thickness of 30 nm and a refractive index of 2.15.

[0077] Then, 4000 ammonia, 1000 silane and 7000 nitrous oxide were introduced, the RF power was 10000 W, the pressure was 1300 mT, and the process time was 80 s; a SiONx film was prepared with a film thickness of 30 nm and a refractive index of 1.7.

[0078] Example 4

[0079] The difference from Example 1 is: The operating temperature for preparing the first anti-reflection film layer on the front side is 470°C, and the operating temperature for preparing the second anti-reflection film layer on the back side is 470°C.

[0080] Comparative Example 1

[0081] The difference from Example 1 is: The cleaned substrate was placed in the ALD equipment, the operating temperature of the equipment was set to 240°C, water was introduced for 6000ms, TMA was introduced for 6000ms after waiting for purge, and then waiting for purge, alternating the chamber reaction, and after 62 cycles of passivation, an aluminum oxide layer with a thickness of 8.2mm was prepared.

[0082] Comparative Example 2

[0083] The difference from Example 1 is: The cleaned substrate was placed in the ALD equipment, the operating temperature of the equipment was set to 240°C, water was introduced for 6000ms, TMA was introduced for 6000ms after waiting for purge, and then waiting for purge, alternating the chamber reaction, and after 18 cycles of passivation, an aluminum oxide layer with a thickness of 2.2mm was prepared.

[0084] Comparative Example 3

[0085] The difference from Example 1 is: The preparation method of the bottom anti-reflection film layer of the first anti-reflection film layer on the front side is as follows: introducing 6000 ammonia and 3000 silane; the RF power is 10000W, the pressure is 1200mT, and the process time is 110s; and a SiNx film is prepared with a film thickness of 20nm and a refractive index of 2.40.

[0086] Comparative Example 4

[0087] The difference from Example 1 is: The preparation method of the bottom anti-reflection film layer of the first anti-reflection film layer on the front side is as follows: introducing 28600 ammonia and 2200 silane; the RF power supply power is 10000W, the pressure is 1300mT, and the process time is 80s; and a SiNx film is prepared with a film thickness of 20nm and a refractive index of 1.9.

[0088] Table 1 below shows the UV-induced attenuation data of Examples 1-4 and Comparative Examples 1-4. It can be seen from the table that (1) compared with Comparative Examples 1-4, the UV-induced attenuation of Examples 1-4 at 15kw, 30kw and 60kw is significantly reduced. (2) The UV-induced attenuation of Examples 1-4 at 15kw is less than 0.7%; the UV-induced attenuation at 30kw is less than 1%; and the UV-induced attenuation at 60kw is less than 2%. (3) Compared with Examples 1-2, Example 3 adopts a stacked structure of SiNx / SiNx / SiONx films and combines the thickness setting of aluminum oxide, and its UV-induced attenuation at 15kw, 30kw and 60kw is further improved; (4) In Example 4, when preparing the first anti-reflection film on the front side and the second anti-reflection film on the back side, the temperature is relatively low, so that the induced attenuation at 60KW becomes higher.

[0089] Table 1 UV-induced attenuation data of Examples 1-4 and Comparative Examples 1-4 Although the present application is described herein in conjunction with various embodiments, in the process of implementing the claimed application, those skilled in the art may understand and implement other changes to the disclosed embodiments by viewing the drawings, the disclosure, and the appended claims. In the claims, the word "comprising" does not exclude other components or steps, and "one" or "an" does not exclude multiple situations. A single processor or other unit may implement several functions listed in a claim. Certain measures are recorded in different dependent claims, but this does not mean that these measures cannot be combined to produce good results.

[0090] Although the present application has been described in conjunction with specific features and embodiments thereof, it is obvious that various modifications and combinations may be made thereto without departing from the spirit and scope of the present application. Accordingly, this specification and the drawings are merely exemplary illustrations of the present application as defined by the appended claims, and are deemed to have covered any and all modifications, variations, combinations or equivalents within the scope of the present application. Obviously, those skilled in the art may make various modifications and variations to the present application without departing from the spirit and scope of the present application. Thus, if these modifications and variations of the present application fall within the scope of the claims of the present application and their equivalents, the present application is also intended to include these modifications and variations.

Claims

1. A method for preparing a Topcon battery, characterized in that: The method comprises: Step 1: providing a substrate, wherein the substrate comprises a front side and a back side opposite to each other, and performing a texturing treatment on the substrate; Step 2: performing boron diffusion on the substrate; forming a P+ layer on the front side of the substrate; Step 3: cleaning and polishing the back side of the substrate, passivating it with a silicon dioxide film and an amorphous silicon layer, and then performing phosphorus doping to form an N+ layer; Step 4: Clean the front side of the substrate to remove the front side plating; and form an aluminum oxide layer with a thickness of 3-6 nm on the P+ layer; Step 5: depositing a first anti-reflection film layer and a second anti-reflection film layer on the front side of the substrate and the back side of the substrate respectively; wherein the first anti-reflection film layer comprises at least one layer, and the refractive index of the bottom anti-reflection film layer of the first anti-reflection film layer close to the aluminum oxide layer is 2.08-2.30; Step 6: Perform printing and drying treatments on the front side and the back side of the substrate respectively.

2. The preparation method according to claim 1, characterized in that In step 4, ALD is used to prepare the aluminum oxide layer, wherein water is introduced for 4000-7000 ms at a temperature of 230-300°C, TMA is introduced for 4000-7000 ms after waiting for purge, and then TMA and water are alternately introduced into the cavity and the silicon wafer for reaction while waiting for purge, and the aluminum oxide layer is obtained after 25-45 cycles of passivation.

3. The preparation method according to claim 1, characterized in that: In the step 5, PECVD is used to prepare the first anti-reflection film layer and the second anti-reflection film layer, wherein the operating temperature of PECVD for preparing the first anti-reflection film is greater than the operating temperature of PECVD for preparing the second anti-reflection film.

4. The preparation method according to claim 3, characterized in that: The operating temperature when preparing the first anti-reflection film is 480-540°C; the operating temperature when preparing the second anti-reflection film is 470-520°C.

5. The preparation method according to claim 1, characterized in that: The bottom anti-reflection film layer is a SiNx film, and / or the thickness of the bottom anti-reflection film layer is 10-20 nm.

6. The preparation method according to claim 5, characterized in that: The method for preparing the bottom anti-reflection film layer is: introducing 6000-12000sccm of ammonia, 1000-3000sccm of silane, 5000-15000W of RF power, 1300mT-2000mT of pressure, and 50-200s of process time.

7. The preparation method according to claim 6, characterized in that: The method for preparing the bottom anti-reflection film layer is: introducing silane and ammonia in a ratio of 1:3 to 1:

5.

8. The preparation method according to claim 1, characterized in that: The first anti-reflection film layer includes at least two layers, the bottom anti-reflection film layer is a SiNx film, and the other layers are SiNx films, SiONx films or SiOx films.

9. The preparation method according to claim 8, characterized in that: The sub-bottom anti-reflection film layer arranged on the bottom anti-reflection film layer is a SiNx film, and / or the refractive index of the sub-bottom anti-reflection film layer is 2.15~2.25; and / or the thickness of the sub-bottom anti-reflection film layer is 20~30nm; and / or the method for preparing the sub-bottom anti-reflection film layer is: the ratio of silane and ammonia introduced is 1:5~1:

12.

10. The preparation method according to claim 9, characterized in that: The film arranged on the sub-bottom anti-reflection film layer is a SiONx film; and / or, the refractive index of the SiONx film is 1.7-1.95; and / or, the thickness of the SiONx film layer is 10-40nm; and / or, the method for preparing the SiONx film is: the ratio of introducing silane, ammonia and nitrous oxide is 1: (3-6): (7-10).

11. A Topcon battery, characterized in that: The product is prepared by the preparation method according to any one of claims 1 to 10.

12. A photovoltaic module, characterized in that: Comprising the Topcon battery of claim 11.

13. A photovoltaic system, characterized in that: A photovoltaic module comprising the photovoltaic module according to claim 12.

Citation Information

Patent Citations

  • N-type double-faced solar cell and preparation method thereof

    CN106409989A

  • Solar cell, preparation method thereof and photovoltaic module

    CN117525180A

  • Preparation method of Topcon battery

    CN117525211A

  • Double-sided TOPCon battery structure for preparing electrodes by adopting electrochemical deposition method and process method of double-sided TOPCon battery structure

    CN118136700A

  • High-efficiency back junction cell structure and preparation method thereof

    CN118472068A