Polybenzimidazole proton exchange membrane with cross-linked structure as well as preparation method and application of polybenzimidazole proton exchange membrane
By using polybenzimidazole molecular chains interspersed in the cross-linking network structure of imidazole compounds and epoxy compounds in high-temperature proton exchange membranes, and protecting imidazole groups through transition metal complexing, the imidazole group consumption in the prior art is solved. The problem of reducing proton conductivity has achieved more stable mechanical properties and efficient phosphoric acid doping.
Patent Information
- Application Number
- CN202410999794.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-15
AI Technical Summary
The existing high-temperature proton exchange membrane consumes imidazole groups during crosslinking, resulting in a decrease in proton conductivity and affecting the mechanical stability and performance of the membrane.
The cross-linking network structure is constructed by interspersing polybenzimidazole molecular chains into an imidazole compound and epoxy compound, and the imidazole group is protected by transition metal complexing to avoid its consumption during cross-linking, forming a proton exchange with a cross-linking structure. membrane.
The mechanical properties and phosphoric acid doping amount of the membrane are improved, the proton conductivity of the high-temperature proton exchange membrane is maintained, the volume swelling rate is reduced, and the stability and performance of the membrane are enhanced.
Smart Images

Figure CN118970122A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fuel cell proton exchange membranes, and in particular relates to a polybenzimidazole proton exchange membrane with a cross-linked structure and a preparation method and application thereof. Background Art
[0002] In the context of the global transition to low-carbon energy, high-temperature proton exchange membrane fuel cells (HTPEMFCs) have developed rapidly due to their high operating temperature, high tolerance of catalysts to impurities such as CO, and simple water and heat management systems. As the core component of HTPEMFCs, high-temperature proton exchange membranes have an important impact on the operating temperature, performance, life, and system cost of fuel cells. At present, anhydrous phosphoric acid system membranes represented by polybenzimidazole PBI are the most recognized and fastest industrialized high-temperature proton exchange membranes in the market. However, after polybenzimidazole membranes absorb phosphoric acid, due to the plasticization of phosphoric acid, the membrane has a large swelling degree and a significant decrease in mechanical strength, which greatly affects the battery performance of the membrane. To address this problem, people choose to modify PBI by chemical cross-linking technology to reduce the dimensional swelling of the membrane after acid doping, thereby improving the dimensional stability and mechanical stability of the membrane. Traditional cross-linking agents contain bifunctional or multifunctional groups, which react with the imine groups in the PBI molecular structure to undergo cross-linking reactions. In this cross-linking process, the imidazole groups of the PBI polymer need to be consumed, resulting in a decrease in the phosphoric acid doping level of the membrane after cross-linking, leading to a decrease in proton conductivity. Summary of the invention
[0003] The purpose of the present invention is to provide a polybenzimidazole proton exchange membrane with a cross-linked structure and a preparation method and application thereof, so as to solve the technical problem that the proton conductivity of the existing exchange membrane is reduced due to consumption of imidazole groups during the preparation process.
[0004] In order to achieve the above object, the present invention adopts the following technical solutions:
[0005] The present invention discloses a polybenzimidazole proton exchange membrane with a cross-linked structure, wherein the microstructure of the exchange membrane is composed of polybenzimidazole molecular chains interlaced in a cross-linked network structure;
[0006] The cross-linked network structure is constructed by an imidazole compound and an epoxy compound;
[0007] The imidazole groups in the polybenzimidazole molecular chain are complexed with transition metals.
[0008] Furthermore, the thickness of the polybenzimidazole proton exchange membrane with a cross-linked structure is 35-45 microns.
[0009] The present invention also discloses a method for preparing the polybenzimidazole proton exchange membrane having a cross-linked structure, comprising the following steps:
[0010] Using polybenzimidazole and transition metal halide as raw materials, preparing a polybenzimidazole modified solution;
[0011] The polybenzimidazole modified solution, the imidazole compound and the epoxy compound are mixed, and stirred, cast into a film and cross-linked in sequence to obtain a cross-linked polybenzimidazole film;
[0012] The transition metal ions are removed from the cross-linked polybenzimidazole membrane, and then water removal and drying are performed in sequence to obtain a polybenzimidazole proton exchange membrane with a cross-linked structure.
[0013] Furthermore, the steps of preparing the polybenzimidazole modified solution using polybenzimidazole and transition metal halide as raw materials are as follows:
[0014] The polybenzimidazole is dissolved in an organic solvent and stirred under an inert atmosphere to obtain a mixed solution; then a transition metal halide is added to the mixed solution for reaction, and after the reaction, the mixture is filtered and the solvent is removed from the obtained liquid component to obtain a polybenzimidazole modified solution.
[0015] Furthermore, the stirring is carried out at 50-80° C. under an inert atmosphere to obtain a mixed solution with a mass fraction of 2%-4%; the reaction temperature is 50-70° C., and the reaction time is 6-10 hours;
[0016] The liquid component is subjected to reduced pressure distillation to remove part of the solvent to obtain a polybenzimidazole modified solution with a mass fraction of 8%-10%;
[0017] The molar ratio of the transition metal halide to the imidazole group in the polybenzimidazole is (0.1-0.4):1.
[0018] Furthermore, the polybenzimidazole is one or more polymers containing benzimidazole structural units in the main chain;
[0019] The organic solvent is one or more of dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide and N-methylpyrrolidone;
[0020] The chemical formula of the transition metal halide is MX2, wherein M is one of copper, nickel and cobalt, and X is one of chlorine and bromine.
[0021] Further, the polybenzimidazole modified solution, the imidazole compound and the epoxy compound are mixed, mechanically stirred for 3-5 hours to obtain a casting solution, and then the casting solution is cast into a film, and then the solvent is volatilized at 70-90° C. and cross-linked to obtain a cross-linked polybenzimidazole film;
[0022] The imidazole compound is a compound containing an imidazole structure;
[0023] The compound containing an imidazole structure is one or more of 2-methylimidazole, 1-benzyl-2-methylimidazole and 1-aminoethyl-2-ethylimidazole;
[0024] The epoxy compound is one or more compositions of bifunctional or trifunctional resins containing epoxy structures.
[0025] Furthermore, the molar ratio of the imidazole compound to the polybenzimidazole is (0.01-0.1):1;
[0026] The molar ratio of the epoxy group of the epoxy compound to the imidazole group of the imidazole compound is 1.2:1;
[0027] The epoxy compound is one or more of bisphenol A, bisphenol F and biphenyl epoxy resin; the viscosity of the epoxy compound is 300-1500 mPaS.
[0028] Furthermore, the cross-linked polybenzimidazole membrane removes transition metal ions and residual solvent by placing the cross-linked polybenzimidazole membrane in deionized water for removal; the temperature of the deionized water is above 80°C;
[0029] The dehydration method is vacuum drying for dehydration; the temperature of vacuum drying for dehydration is 120°C and the time is 4-6h;
[0030] The drying process is carried out at a temperature of 160-180° C. and for a time of 2-3 hours.
[0031] The invention also discloses the application of the polybenzimidazole proton exchange membrane with a cross-linked structure in a high-temperature fuel cell.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] The invention discloses a polybenzimidazole proton exchange membrane with a cross-linked structure. An imidazole network structure with a structure similar to that of polybenzimidazole is designed, and polybenzimidazole molecular chains are interspersed in a cross-linked network structure of an imidazole compound and an epoxy compound. The cross-linked network structure not only fixes the polybenzimidazole molecular chains in the structure, but also has good intermolecular forces with the polybenzimidazole, thereby effectively solving the problem of traditional cross-linking agents consuming the polybenzimidazole structure. The imidazole groups in the polybenzimidazole polymer structure are complexed with transition metals, thereby increasing the cross-linking temperature of the imidazole functional groups and epoxy groups in the polybenzimidazole molecular chain structure, and do not participate in the construction of the cross-linked network, thereby avoiding the consumption of the imidazole structure.
[0034] The present invention also discloses a method for preparing the above-mentioned polybenzimidazole proton exchange membrane with a cross-linked structure, which comprises complexing polybenzimidazole with transition metal ions to protect the imidazole group, cross-linking at 70-90°C by adding an imidazole compound and an epoxy compound to construct a network, then removing the transition metal ions and residual solvents by deionized water, and drying to obtain a cross-linked polybenzimidazole membrane. The method is simple to prepare and has good application prospects.
[0035] The present invention also discloses the application of the polybenzimidazole proton exchange membrane with a cross-linked structure in a high-temperature fuel cell. According to relevant experimental results, it is proved that by soaking the cross-linked polybenzimidazole membrane material in 85% by mass phosphoric acid at 100-120° C. for 8h-12h, the phosphoric acid is fully absorbed by the cross-linked polybenzimidazole membrane material, and a polybenzimidazole proton exchange membrane wet membrane with a phosphoric acid doping amount of 350-450% can be obtained; it is proved that without reducing the PBI imidazole content, the obtained cross-linked high-temperature proton exchange membrane has good mechanical properties and a low volume swelling rate after adsorbing phosphoric acid. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 Comparison of solubility tests of sample films of Example 1 and different comparative examples;
[0037] Wherein: a-Example 1; b-Comparative Example 1; c-Comparative Example 2; d-Comparative Example 3;
[0038] Figure 2 is the DSC test curve of the polybenzimidazole film with cross-linking reaction;
[0039] Figure 3 This is the battery performance test curve for preparing polybenzimidazole proton membrane. DETAILED DESCRIPTION
[0040] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0041] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0042] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0043] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”
[0044] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0045] The present invention designs an imidazole network structure with a structure similar to that of polybenzimidazole, wherein the polybenzimidazole molecular chains are interspersed in a cross-linked network structure of imidazole compounds and epoxy compounds. The network structure not only fixes the polybenzimidazole molecular chains in the structure, but also has good intermolecular forces with the polybenzimidazole.
[0046] The present invention provides a method for preparing the polybenzimidazole proton exchange membrane having a cross-linked structure, comprising the following steps:
[0047] Step 1: Preparation of polybenzimidazole modified solution
[0048] Dissolve polybenzimidazole in an organic solvent, and stir at 50-80° C. under nitrogen protection to fully dissolve to obtain a mixed solution with a mass fraction of 2-4%;
[0049] Dissolve the transition metal halide MX2 in a polar organic solvent and stir at room temperature for 15-30 minutes to obtain a transition metal solution;
[0050] The transition metal halide solution is slowly added dropwise to the mixed solution under stirring, and the mixture is reacted at 50-70° C. for 6-10 hours after the addition is completed. After the reaction is completed, the solid by-products are removed by filtration, and the filtered solution components are distilled under reduced pressure to increase the solute mass fraction to 8%-10%, thereby obtaining a polybenzimidazole modified solution;
[0051] Step 2: Preparation of cross-linked polybenzimidazole membrane
[0052] The obtained polybenzimidazole modified solution is mixed with the imidazole compound and the epoxy compound, and mechanically stirred for 3-5 hours to ensure uniform mixing to obtain a viscous casting solution;
[0053] The casting solution is cast into a film in a casting machine, and the solvent is volatilized and cross-linked for 20-30 minutes at a temperature gradient of 70-90° C. to obtain a cross-linked polybenzimidazole film;
[0054] Step 3: Preparation of polybenzimidazole proton exchange membrane with cross-linked structure
[0055] The cross-linked polybenzimidazole membrane was immersed in 90°C deionized water for 4 hours, during which the water was changed every 1 hour to remove transition metal ions. After the membrane was taken out, the surface water was wiped clean with dust-free paper. It was first placed in a 120°C vacuum oven for vacuum drying and dehydration for 4 hours, and then dried at 160-180°C for 2-3 hours to obtain a polybenzimidazole proton exchange membrane with a cross-linked structure.
[0056] Preferably, the chain structural unit of the polybenzimidazole is a polybenzimidazole with good solubility, preferably one or a mixture of mPBI (weight average molecular weight of about 60,000) or OPBI containing an ether bond (weight average molecular weight of about 100,000).
[0057] Preferably, the transition metal halide MX2, wherein M is copper, nickel or cobalt, and X is chlorine or bromine.
[0058] Preferably, the organic solvent is one or more solvents selected from the group consisting of dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide or N-methylpyrrolidone.
[0059] Preferably, the molar ratio of the transition metal halide to the imidazole group in the polybenzimidazole is (0.1-0.4):1.
[0060] Preferably, the imidazole compound is one or more of 2-methylimidazole, 1-benzyl-2-methylimidazole and 1-aminoethyl-2-ethylimidazole.
[0061] Preferably, the epoxy compound is a small molecule compound or a macromolecular polymer containing a difunctional or trifunctional epoxy group, and the epoxy compound preferably has a viscosity of 300-1000 mPa.s.
[0062] Preferably, the molar ratio of the epoxy group of the epoxy compound to the imidazole structure in the imidazole compound is 1.2:1.
[0063] Preferably, the drying oven temperature is 70-90°C.
[0064] Preferably, the thickness of the polybenzimidazole proton exchange membrane having a cross-linked structure is 35-45 microns.
[0065] The present invention also provides application of the polybenzimidazole proton exchange membrane with a cross-linked structure in a high-temperature fuel cell.
[0066] The present invention also verifies the phosphoric acid absorption performance of the polybenzimidazole proton exchange membrane having a cross-linked structure:
[0067] In the step of immersing the polybenzimidazole proton exchange membrane dry film in phosphoric acid to obtain the polybenzimidazole proton exchange membrane wet film, 85% mass fraction phosphoric acid is used for immersion at 100-120° C. for 8h-12h, so that the cross-linked polybenzimidazole membrane material fully absorbs the phosphoric acid, and the polybenzimidazole proton exchange membrane wet film with a phosphoric acid doping amount of 350-450% can be obtained.
[0068] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0069] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.
[0070] The performance rules of the films prepared from polybenzimidazoles with different structures using the method of the present invention are similar, and a comparative verification is performed by taking OPBI with a weight average molecular weight of 100,000 and mPBI with a weight average molecular weight of 60,000 as examples.
[0071] Example 1
[0072] A method for preparing a polybenzimidazole proton exchange membrane having a cross-linked structure comprises the following steps:
[0073] S1: 40 g (0.1 mol) of polybenzimidazole (OPBI) was dissolved in 960 g of N, N-dimethylacetamide, and fully dissolved at 50° C. under nitrogen gas protection to obtain a mixed solution with a mass fraction of 4%; 4.25 g (0.025 mol) of CuCl2 was dissolved in 10 g of N, N-dimethylacetamide, and stirred at room temperature for 30 min to obtain a CuCl2 solution, and the CuCl2 solution was slowly added dropwise to the mixed solution under stirring conditions. After the addition was completed, the mixture was reacted at 60° C. for 8 hours, and then the solid by-products were filtered out, and the solute content of the solution components obtained by filtration was increased to 10% by vacuum distillation to obtain a polybenzimidazole modified solution;
[0074] S2: The polybenzimidazole modified solution obtained in S1 was mixed with 1.73g 1-benzyl-2-methylimidazole and 2g epoxy resin E51, and mechanically stirred for 4 hours to obtain a viscous casting solution; the casting solution was cast into a film in a casting machine, and passed through a three-stage drying tunnel at a speed of 0.1m / min, and the three-stage temperatures were 60°C, 70°C, and 80°C, respectively, to obtain a cross-linked polybenzimidazole film;
[0075] S3: The cross-linked polybenzimidazole membrane obtained in S2 is immersed in 90°C deionized water for 4 hours, during which the water is changed every 1 hour. After removing the transition metal ions, the membrane surface is wiped clean with dust-free paper, and first dried in a 120°C vacuum oven for 4 hours, and then dried at 160°C for 3 hours to obtain a polybenzimidazole membrane with a cross-linked structure.
[0076] Example 2
[0077] A method for preparing a polybenzimidazole proton exchange membrane having a cross-linked structure comprises the following steps:
[0078] S1: 30 g (0.1 mol) of polybenzimidazole (mPBI) was dissolved in 960 g of N, N-dimethylacetamide, and fully dissolved at 60° C. under nitrogen gas protection to obtain a mixed solution with a mass fraction of 4%; 5.95 g (0.025 mol) of CoCl26H2O was dissolved in 10 g of N, N-dimethylacetamide, and stirred at room temperature for 30 min to obtain a CoCl26H2O solution, and the CoCl26H2O solution was slowly added dropwise to the mixed solution under stirring conditions. After the addition was completed, the mixture was reacted at 60° C. for 8 hours, and then the solid by-products were removed by filtration. The solution components obtained by filtration were subjected to reduced pressure distillation to increase the solute content to 10%, and a polybenzimidazole modified solution was obtained;
[0079] S2: The polybenzimidazole modified solution obtained in S1 was mixed with 1.73g 1-benzyl-2-methylimidazole and 2g epoxy resin E51, and mechanically stirred for 4 hours to obtain a viscous casting solution; the casting solution was cast into a film in a casting machine, and passed through a three-stage drying tunnel at a speed of 0.1m / min, and the three-stage temperatures were 60°C, 70°C, and 80°C, respectively, to obtain a cross-linked polybenzimidazole film;
[0080] S3: The cross-linked polybenzimidazole membrane obtained in S2 is immersed in 90°C deionized water for 4 hours, during which the water is changed every 1 hour. After removing the transition metal ions, the membrane surface is wiped clean with dust-free paper, and first dried in a 120°C vacuum oven for 4 hours, and then dried at 160°C for 3 hours to obtain a polybenzimidazole membrane with a cross-linked structure.
[0081] Example 3
[0082] A method for preparing a polybenzimidazole proton exchange membrane having a cross-linked structure comprises the following steps:
[0083] S1: dissolving polybenzimidazole in dimethyl sulfoxide, fully dissolving at 80°C under nitrogen protection to obtain a mixed solution with a mass fraction of 2%; slowly dropping NiCl2 solution into the mixed solution under stirring conditions, reacting at 70°C for 8 hours after the dropping is completed, then filtering to remove solid by-products, and increasing the solute content of the filtered solution components to 10% by vacuum distillation to obtain a polybenzimidazole modified solution;
[0084] S2: The polybenzimidazole modified solution obtained in S1 is mixed with 1-aminoethyl-2-ethylimidazole and epoxy resin E51, and mechanically stirred for 3 hours to obtain a viscous casting solution; the casting solution is cast into a film in a casting machine, and passed through a three-stage drying tunnel at a speed of 0.1m / min, and the three-stage temperatures are 60°C, 70°C, and 80°C, respectively, to obtain a cross-linked polybenzimidazole film; wherein the molar ratio of the imidazole compound to the polybenzimidazole is 0.01:1, and the molar ratio of the epoxy group of the epoxy compound to the imidazole group in the imidazole compound is 1.2:1;
[0085] S3: The cross-linked polybenzimidazole membrane obtained in S2 is immersed in 90°C deionized water for 4 hours, during which the water is changed every 1 hour. After removing the transition metal ions, the membrane surface is wiped clean with dust-free paper, and first dried in a 120°C vacuum oven for 6 hours, and then dried at 180°C for 2 hours to obtain a polybenzimidazole membrane with a cross-linked structure.
[0086] Comparative Example 1
[0087] The polybenzimidazole modified solution of S1 in Example 1 was mixed with 2g of bisphenol A epoxy resin and mechanically stirred for 4 hours. The casting solution was cast into a film in a casting machine and passed through a three-stage drying tunnel at a speed of 0.1m / min. The three-stage temperatures were 60°C, 70°C, and 80°C, respectively, to obtain a polybenzimidazole film.
[0088] Comparative Example 2
[0089] The polybenzimidazole modified solution of S1 in Example 1 was mixed with 2g of bisphenol A epoxy resin and mechanically stirred for 4 hours. The casting solution was cast into a film in a casting machine and passed through a three-stage drying tunnel at a speed of 0.1m / min. The three-stage temperatures were 95°C, 110°C, and 130°C, respectively, to obtain a polybenzimidazole film containing a transition metal.
[0090] The obtained polybenzimidazole membrane was immersed in 90°C deionized water for 4 hours, during which the water was changed every 1 hour. After removing the transition metal ions, the membrane surface was wiped clean with dust-free paper, and then dried in a vacuum oven at 120°C for 4 hours to obtain the polybenzimidazole membrane.
[0091] Comparative Example 3
[0092] S1: 40 g (0.1 mol) (OPBI) was dissolved in 360 g N,N-dimethylacetamide, and stirred at 60° C. under the protection of an inert gas until fully dissolved to obtain a solution with a mass fraction of 10%.
[0093] S2: The polybenzimidazole solution obtained in S1 was mixed with 2g of bisphenol A epoxy resin and mechanically stirred for 4 hours. The casting solution was cast into a film in a casting machine and passed through a three-stage drying tunnel at a speed of 0.1m / min. The three-stage temperatures were 60°C, 70°C, and 80°C, respectively, to obtain a cross-linked polybenzimidazole film.
[0094] Comparative Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3 were tested for solubility in N,N-dimethylacetamide and dissolved by stirring at 60°C for 2h. The solubility was as follows: Figure 1 , it can be seen that Example 1 is insoluble in the solvent N,N-dimethylacetamide, because the cross-linked network constructed by small molecule imidazole and compound and epoxy group hinders the solubility of polybenzimidazole; the samples of Comparative Examples 2 and Comparative Examples 3 are insoluble in N,N-dimethylacetamide, respectively indicating that after polybenzimidazole is complexed with transition metal (Comparative Example 2), the reaction temperature of imidazole group and epoxy group in polybenzimidazole is increased, and the uncomplexed polybenzimidazole (Comparative Example 3) undergoes cross-linking reaction with epoxy in a 60-80℃ drying oven; most of the sample of Comparative Example 1 is soluble in N,N-dimethylacetamide, and only a trace amount of sample is insoluble (white is a stir bar), indicating that after polybenzimidazole is complexed with transition metal, only very slight cross-linking occurs in a 60-80℃ drying oven, and complexation improves the stability of imidazole group in polybenzimidazole. The entire dissolution test shows by comparison that the polybenzimidazole molecular chain is interspersed in the cross-linked network structure of imidazole compound and epoxy compound.
[0095] The dry film tensile strength, phosphoric acid absorption, tensile strength of the wet film after being soaked in phosphoric acid, and volume swelling rate of the samples in Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3 were tested, and the test results are shown in Table 1; in Table 1, phosphoric acid absorption = (mass of the wet film after absorbing phosphoric acid - mass of the dry film) / mass of the dry film * 100%, and volume swelling rate = (volume of the wet film - volume of the dry film) / volume of the dry film * 100%.
[0096] Table 1 Performance test results of different examples and comparative examples
[0097]
[0098]
[0099] Analyzing Table 1, by comparing the mechanical properties of the two groups of membranes of Example 1 and Comparative Example 1, it can be seen that the tensile strength of the dry membrane of Example 1 with a cross-linked network structure is higher than that of Comparative Example 1 without a cross-linked structure, and the phosphoric acid adsorption of the two samples is almost the same, but the tensile strength of the wet membrane of Example 1 is significantly higher than that of Comparative Example 1, and the volume swelling rate is lower than that of the Comparative Example. Compared with the non-cross-linked membrane of the Comparative Example, the phosphoric acid absorption capacity of the PBI membrane with a cross-linked structure of the embodiment is not reduced, but slightly improved. The reason for this is that the cross-linked network uses an imidazole compound containing a basic site to enhance the adsorption of phosphoric acid; by comparing Example 1, Comparative Example 2, and Comparative Example 3, it can be seen that the tensile strength of the dry membrane of the thin film prepared by interlacing PBI molecular chains in a cross-linked network constructed by imidazole compounds is not much different from that of the thin film prepared by direct cross-linking of PBI and epoxy, but the amount of phosphoric acid adsorption is higher than the latter.
[0100] A small amount of the S2 casting solution in Example 1, the casting solution in Comparative Example 2, and the S2 casting solution in Comparative Example 3 were taken and tested on a differential scanning calorimeter at an isothermal rate of 10°C / min. N,N-dimethylacetamide was selected as the reference sample, and the exothermic peak temperature of the resin crosslinking process was measured respectively. All tests were carried out in nitrogen. Figure 2 It can be seen from the DSC diagram that Example 1 absorbs heat from 60°C, indicating that the cross-linking reaction begins to proceed, and the heat release reaches a maximum at 82°C; Comparative Example 2 begins to absorb heat from 82°C, and the heat release reaches a maximum at ~120°C, indicating that the complexation of polybenzimidazole with transition metal ions increases the polymerization temperature of imidazole groups and epoxy groups, and also shows that below 80°C, the complex only slightly reacts with the epoxy resin, which is consistent with the solubility experiment of Comparative Example 1 in N,N-dimethylacetamide; Comparative Example 3 absorbs heat from 60°C, and since polybenzimidazole is not complexed with the transition metal, the cross-linking reaction of the polymer imidazole groups and the epoxy groups begins to release heat.
[0101] The sample membranes of Example 1, Comparative Example 1 and Comparative Example 3 were subjected to battery performance tests. In the single-cell test, 0.3 L / min hydrogen and 0.5 L / min air were supplied without back pressure. The test temperature was 160°C. The carbon paper used was 060 type carbon paper produced by Toray. The platinum loading of the cathode and anode electrodes was 0.5 mg / cm 2 , the results are as follows Figure 1 ;Depend on Figure 3 It can be seen that the peak power density of the membrane electrode assembled using the PBI proton membrane prepared using the imidazole epoxy cross-linked network (Example 1) is higher than that of Comparative Example 1 and Comparative Example 3, indicating that the proton membrane of the present invention has excellent performance in practical applications of batteries.
[0102] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A polybenzimidazole proton exchange membrane having a cross-linked structure, characterized in that: The microstructure of the exchange membrane is composed of polybenzimidazole molecular chains interlaced in a cross-linked network structure; The cross-linked network structure is constructed by an imidazole compound and an epoxy compound; The imidazole groups in the polybenzimidazole molecular chain are complexed with transition metals.
2. The polybenzimidazole proton exchange membrane with a cross-linked structure according to claim 1, characterized in that: The thickness of the polybenzimidazole proton exchange membrane with a cross-linked structure is 35-45 microns.
3. The method for preparing a polybenzimidazole proton exchange membrane having a cross-linked structure according to claim 1 or 2, characterized in that: The following steps are involved: Using polybenzimidazole and transition metal halide as raw materials, preparing a polybenzimidazole modified solution; The polybenzimidazole modified solution, the imidazole compound and the epoxy compound are mixed, and stirred, cast into a film and cross-linked in sequence to obtain a cross-linked polybenzimidazole film; The transition metal ions are removed from the cross-linked polybenzimidazole membrane, and then water removal and drying are performed in sequence to obtain a polybenzimidazole proton exchange membrane with a cross-linked structure.
4. The method for preparing a polybenzimidazole proton exchange membrane having a cross-linked structure according to claim 3, characterized in that: The steps of preparing the polybenzimidazole modified solution using polybenzimidazole and transition metal halide as raw materials are as follows: The polybenzimidazole is dissolved in an organic solvent and stirred under an inert atmosphere to obtain a mixed solution; then a transition metal halide is added to the mixed solution for reaction, and after the reaction, the mixture is filtered and the solvent is removed from the obtained liquid component to obtain a polybenzimidazole modified solution.
5. The method for preparing a polybenzimidazole proton exchange membrane having a cross-linked structure according to claim 4, characterized in that: The stirring at 50-80° C. under an inert atmosphere to obtain a mixed solution with a mass fraction of 2%-4%; the reaction temperature is 50-70° C. and the reaction time is 6-10 hours; The liquid component is subjected to reduced pressure distillation to remove part of the solvent to obtain a polybenzimidazole modified solution with a mass fraction of 8%-10%; The molar ratio of the transition metal halide to the imidazole group in the polybenzimidazole is (0.1-0.4):
1.
6. The method for preparing a polybenzimidazole proton exchange membrane having a cross-linked structure according to claim 5, characterized in that: The polybenzimidazole is one or more polymers containing benzimidazole structural units in the main chain; The organic solvent is one or more of dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide and N-methylpyrrolidone; The chemical formula of the transition metal halide is MX2, wherein M is one of copper, nickel and cobalt, and X is one of chlorine and bromine.
7. The method for preparing a polybenzimidazole proton exchange membrane having a cross-linked structure according to claim 3, characterized in that: The polybenzimidazole modified solution, the imidazole compound and the epoxy compound are mixed and mechanically stirred for 3-5 hours to obtain a casting solution, and then the casting solution is cast into a film, and then the solvent is volatilized at 70-90° C. and cross-linked to obtain a cross-linked polybenzimidazole film; The imidazole compound is a compound containing an imidazole structure; The compound containing an imidazole structure is one or more of 2-methylimidazole, 1-benzyl-2-methylimidazole and 1-aminoethyl-2-ethylimidazole; The epoxy compound is one or more compositions of bifunctional or trifunctional resins containing epoxy structures.
8. The method for preparing a polybenzimidazole proton exchange membrane having a cross-linked structure according to claim 7, characterized in that: The molar ratio of the imidazole compound to the polybenzimidazole is (0.01-0.1):1; The molar ratio of the epoxy group of the epoxy compound to the imidazole group of the imidazole compound is 1.2:1; The epoxy compound is one or more of bisphenol A, bisphenol F and biphenyl epoxy resin; the viscosity of the epoxy compound is 300-1500 mPaS.
9. The method for preparing a polybenzimidazole proton exchange membrane having a cross-linked structure according to claim 3, characterized in that: The cross-linked polybenzimidazole membrane removes transition metal ions and residual solvent by placing the cross-linked polybenzimidazole membrane in deionized water for removal; the temperature of the deionized water is above 80°C; The dehydration method is vacuum drying for dehydration; the temperature of vacuum drying for dehydration is 120°C and the time is 4-6h; The drying process is carried out at a temperature of 160-180° C. and for a time of 2-3 hours.
10. Use of the cross-linked polybenzimidazole proton exchange membrane according to claim 1 or 2 in a high-temperature fuel cell.
Citation Information
Cited By
Polybenzimidazole modified ion conducting membrane for flow battery and preparation method of polybenzimidazole modified ion conducting membrane
CN121181962A