Attaching method of vacuum plate lining
Through the adhesion method of vacuum board lining, ultra-fine composite grinding and high-pressure steam are used to solve the problem of secondary pollution of wet electronic chemicals in the production process, high-purity product output is achieved, and metal ion impurities content is reduced. , and improves productivity and economic benefits.
Patent Information
- Application Number
- CN202411363764.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-28
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-09-28
AI Technical Summary
During the production process, wet electronic chemicals are easily contaminated by metal ions and solid particles in the inner walls of equipment and pipelines, resulting in secondary pollution, affecting product purity and the electrical performance of the chip.
Adopting methods of vacuum board lining, including ultra-fine composite polishing, non-woven fabric glue, special board lining materials and high-pressure steam drum sticking installation, combined with vacuuming operation, prevent metal ions and particles from infiltration, and use ultra-pure nitrogen Cover to avoid secondary contamination.
Effectively block the infiltration of metal ions and particulate matter in the inner wall of the equipment and pipeline, significantly improve the purity of chemical products, reduce the content of metal ion impurities to below 5ppt, extend the life of the board lining, and improve the production efficiency and economic benefits of wet electronic chemicals.
Smart Images

Figure CN118977503A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of chemical equipment manufacturing, and more particularly to a method for attaching a vacuum plate lining. Background Art
[0002] Wet electronic chemicals are widely used in the cleaning, photolithography, development, etching, doping and other process links of micro-fabrication of electronic components such as chips, display panels, solar cells, LEDs, etc. In "chip" manufacturing, wet electronic chemicals can effectively remove residual pollutants on the surface of wafers, reduce the content of metal impurities, and provide quality assurance for downstream products.
[0003] Distillation technology and absorption technology are common and key technologies for chemical purification, and are also indispensable technologies in the preparation of wet electronic chemicals. During the preparation of wet electronic chemicals, materials are easily contaminated when in contact with tower equipment, tank equipment, pump equipment, pipelines, etc., thus affecting the purity of wet electronic chemicals.
[0004] In order to ensure the yield of "chips", wet electronic chemicals have extremely high requirements for metal ions and solid particles, with a content of ppt, which is equivalent to dropping a drop of ink into a standard swimming pool, which is 200 times higher than the standard. Trace metal impurities will seriously affect the electrical properties of the chip and reduce its reliability. In the entire production process of wet electronic chemicals, all equipment and pipe inner walls that the materials come into contact with will inevitably cause secondary pollution of wet electronic chemicals.
[0005] Therefore, how to avoid secondary contamination of wet electronic chemicals is an urgent problem that technicians in this field need to solve. Summary of the invention
[0006] In view of this, an object of the present invention is to provide a method for attaching a vacuum panel liner to solve the deficiencies in the prior art.
[0007] In order to achieve the above object, the present invention adopts the following technical solution:
[0008] A method for attaching a vacuum lining, characterized in that it specifically comprises the following steps:
[0009] (1) Perform ultra-fine composite grinding and polishing on the workpiece to be processed (steel or container);
[0010] (2) Apply glue to the wall surface of the workpiece to be processed and connect the non-woven fabric;
[0011] (3) Apply glue on the surface of the non-woven fabric to connect the board lining material;
[0012] (4) Ultrapure nitrogen is continuously introduced during ultrafine composite grinding and polishing, glue coating, and connecting non-woven fabrics and connecting plate lining materials, and high-pressure steam is continuously introduced during connecting non-woven fabrics and connecting plate lining materials;
[0013] (5) A vacuum operation is performed between the inner wall of the workpiece to be processed and the plate lining material.
[0014] Furthermore, in the above step (1), the ultra-fine composite grinding and polishing includes at least one of ultrasonic grinding, magnetic grinding, chemical grinding and mechanical grinding.
[0015] Furthermore, the ultrasonic grinding is specifically as follows: placing the workpiece to be processed in an ultrasonic environment, and the ultrasonic wavelength λ is 0.02-2 cm.
[0016] A further beneficial effect of the above method is that loose burrs and particles on the wall surface of the workpiece to be processed are removed by using ultrasonic waves.
[0017] Furthermore, the above-mentioned magnetic grinding is specifically as follows: high-performance grinding and polishing materials such as silicon nitride grinding balls, silicon carbide, diamonds, and resins are filled into the workpiece to be processed, and the workpiece to be processed is passed through by a fluid, and rotated at a certain speed while vibrating axially, and a strong DC magnetic field is applied in a plane direction perpendicular to the axis of the workpiece to be processed and the electric lines.
[0018] A further beneficial effect of the above method is that the "abrasive brush" composed of magnetic abrasives quickly impacts the surface of the workpiece to be processed to remove particles and crystals.
[0019] Furthermore, the chemical polishing mentioned above specifically includes: placing the workpiece to be processed in an electrolyte environment and passing electric current to perform electrochemical treatment.
[0020] A further beneficial effect of the above-mentioned method is that the anode of the current and voltage is connected to the burr crystallized part of the workpiece to be processed, and the cathode is connected to a conductive tool with abrasive particles. The electrolyte is driven by a pump and flows through the cathode to the anode to the burr crystallized part of the workpiece to be processed to reach the reflux tank, which can accurately remove the burrs, smooth the surface of the workpiece to be processed, and control the surface roughness Ra of the workpiece to be processed to be 0.2-2μm.
[0021] Furthermore, in the above steps (2) and (3), the glue is at least one of an easily film-forming adhesive such as acrylic acid, a modified copolymer emulsion of acrylic acid and vinyl acetate, and a hot melt adhesive film.
[0022] A further beneficial effect of the above method is that the non-woven fabric is coated with glue on both the inner and outer surfaces, and different types of glue are selected according to the wall material and lining material of the workpiece to be processed, so as to strongly adhere to the wall and the lining.
[0023] Furthermore, in the above step (2), the non-woven fabric is at least one of polypropylene, polyester, natural fiber and chemical fiber.
[0024] Furthermore, in the above step (3), the plate lining material is an alloy containing at least one of chromium, manganese and molybdenum, and is subjected to a quenching process, and the surface roughness Ra is below 10 μm.
[0025] A further beneficial effect of adopting the above method is that the lining surface of the plate lining material selected in the present invention that contacts chemicals is smooth, the plate lining material treated by the quenching process is wear-resistant and corrosion-resistant, does not release pollutants that are harmful to the material, and the side that contacts the non-woven fabric strongly adheres to the non-woven fabric, which can effectively prevent metal ions and particulate matter on the wall of the workpiece to be treated from penetrating into the material.
[0026] Furthermore, in the above step (4), the gauge pressure of the high-pressure steam is 10 to 200 kPa.
[0027] The further beneficial effect of the above method is that ultrapure nitrogen is introduced into the ultra-fine composite grinding and polishing process, the non-woven fabric and the internal and external gluing process, and the lining installation process to avoid the introduction of secondary pollution. High-pressure steam is continuously introduced during the installation of the non-woven fabric and the lining to accelerate the attachment of the non-woven fabric and the lining to the glue. At the same time, the high-pressure steam ensures the flatness, smoothness and integrity of the installation of the non-woven fabric and the lining, so that the maximum height Rz of the installation profile is less than 5μm.
[0028] Furthermore, in the above step (5), the vacuum is evacuated until the absolute pressure of the gap is 30 to 98 kPa.
[0029] A further beneficial effect of the above method is that vacuuming is performed on the gaps of the non-woven fabric connection, so that the connection between the lining and the inner wall of the workpiece to be processed is tighter, the lining is prevented from falling off, the impurity content and mass transfer driving force are reduced, and the penetration of metal ions and particulate matter is prevented.
[0030] It can be seen from the above technical solution that compared with the prior art, the beneficial effects of the present invention are as follows:
[0031] 1. The present invention uses ultra-fine composite grinding technology, and utilizes ultrasonic, magnetic, chemical and mechanical methods to grind the inner wall of the workpiece to be processed, so as to efficiently remove burrs and crystals on the inner wall, and reduce the release of metal ions and particulate matter from the source. At the same time, the ultra-fine composite grinding and polishing technology is more efficient than a single grinding technology, and can grind burrs or crystals while ensuring the smoothness and flatness of the inner wall, and avoid introducing secondary burrs or crystals; adopts special non-woven fabrics with internal and external glue to strongly adhere to the lining layer; develops special plate lining materials with smooth and precise surface, wear resistance and corrosion resistance, and prevents impurities such as metal ions and solid particles from penetrating; proposes a new process for high-pressure steam drum pasting installation to ensure the blocking effect of the lining; vacuumizes the space between the inner wall of the equipment and the plate lining to prevent the penetration of metal ions on the equipment and pipeline walls and the shedding of the lining layer; the non-woven fabric internal and external glue method and the non-woven fabric gap vacuumization technology adopted double guarantee the connection between the inner wall and the lining cloth, greatly prolongs the life of the plate lining of the present invention, and saves costs; ultra-pure nitrogen sealing film is used to avoid secondary pollution during transportation.
[0032] 2. The present invention achieves effective blocking of the infiltration of metal ions and particulate matter on the wall of the workpiece to be processed, and greatly improves the purity of chemicals by performing technical operations such as ultra-fine grinding of the wall of the workpiece to be processed, strong adhesion of the non-woven fabric inside and outside with glue, development of special board lining materials, high-pressure steam drum pressing and installation, vacuum operation between the inner wall of the equipment and the lining layer, and ultra-pure nitrogen sealing and coating.
[0033] 3. The high-strength attached vacuum plate lining technology adopted in the present invention is a special technology with the characteristics of corrosion resistance, wear resistance, high temperature resistance, chemical corrosion resistance, etc. It can effectively block the penetration of metal ions and particulate matter into the inner wall of equipment and pipelines during the production process of wet electronic chemicals, greatly improve the purity of chemical products, and meet the production requirements of G5-level wet electronic chemicals. It creatively reduces the content of various metal ion impurities to below 5ppt, significantly improves economic benefits, and accelerates the production process of high-purity high-end chemicals. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a schematic diagram of ultra-fine composite grinding and polishing;
[0035] Figure 2 Schematic diagram of the vacuum plate lining attachment method. DETAILED DESCRIPTION
[0036] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] Example 1
[0038] Vacuum lining attachment method, such as Figure 1 and Figure 2 As shown, the specific steps include:
[0039] (1) Performing ultra-fine composite grinding and polishing on the workpiece to be processed;
[0040] Ultrasonic grinding and magnetic grinding are adopted. The magnetic pole and ultrasonic source are strengthened in the plane direction perpendicular to the axis of the workpiece to be processed and the electric lines. The ultrasonic wavelength λ is controlled to 2cm to remove the loose burrs and particles on the wall surface. Silicon nitride grinding balls are filled into the workpiece to be processed, flowing through the wall surface along the axis direction, and cutting the magnetic flux lines in the form of axial and rotational motion, stirring the magnetic abrasive in the high-performance grinding and polishing material to grind the wall surface and remove burrs and crystals.
[0041] (2) coating acrylic glue on the wall surface of the workpiece to be processed and connecting the polypropylene non-woven fabric;
[0042] (3) coating acrylic glue on the surface of the polypropylene non-woven fabric to connect the chromium-manganese alloy plate lining material;
[0043] (4) Ultrapure nitrogen was continuously introduced during ultrafine composite grinding and polishing, coating of acrylic glue, connection of polypropylene non-woven fabric and connection of chrome-manganese alloy plate lining materials, and high-pressure steam with a gauge pressure of 10 kPa was continuously introduced during connection of polypropylene non-woven fabric and connection of chrome-manganese alloy plate lining materials;
[0044] (5) The inner wall of the workpiece to be processed and the plate lining material are evacuated until the absolute pressure of the gap is 30 kPa.
[0045] Example 2
[0046] Vacuum lining attachment method, such as Figure 1 and Figure 2 As shown, the specific steps include:
[0047] (1) Performing ultra-fine composite grinding and polishing on the workpiece to be processed;
[0048] Chemical grinding and magnetic grinding are adopted, the anode of the applied voltage is connected to the inner wall of the workpiece with burrs and crystals to be processed, the cathode of the applied voltage is connected to silicon carbide, and the silicon carbide flows through the wall along the axis direction of the workpiece to electrolytically remove the burrs and crystals on the inner wall, so as to achieve the leveling of the wall of the workpiece to be processed;
[0049] (2) coating acrylic glue on the wall surface of the workpiece to be processed and connecting the polypropylene non-woven fabric;
[0050] (3) coating acrylic glue on the surface of the polypropylene non-woven fabric to connect the chromium-manganese alloy plate lining material;
[0051] (4) Ultrapure nitrogen is continuously introduced during ultrafine composite grinding and polishing, coating of acrylic glue, connection of polypropylene non-woven fabric and connection of chrome-manganese alloy plate lining materials, and high-pressure steam with a gauge pressure of 200 kPa is continuously introduced during connection of polypropylene non-woven fabric and connection of chrome-manganese alloy plate lining materials;
[0052] (5) The inner wall of the workpiece to be processed and the plate lining material are evacuated until the absolute pressure of the gap is 98 kPa.
[0053] Performance Testing
[0054] All equipment and pipeline inner walls that come into contact with materials in the entire process of electronic-grade hydrofluoric acid production are lined with vacuum plates according to the methods of Example 1 and Example 2, respectively, and the particle content and metal ion content in the electronic-grade hydrofluoric acid product are detected.
[0055] The particle content detection adopts scanning electron microscope-X-ray energy dispersive spectroscopy (SEM-EDX), which specifically includes the following steps:
[0056] 1. Preliminary preparation
[0057] 1. Check whether the connections of power supply, cooling water, vacuum pump and other equipment are normal, and ensure that the voltage is stable and meets the equipment requirements.
[0058] 2. Place the prepared sample on the sample stage, ensure that the sample is in good contact with the table, and fix it with conductive tape or clamps if necessary. Place the sample stage with the sample into the sample chamber of the SEM and close the sample chamber door.
[0059] 2. Vacuuming and equipment startup
[0060] 1. Use a vacuum pump to extract the air in the sample chamber to achieve the vacuum degree required by the equipment (usually less than 10 -3 Pa).
[0061] 2. Start the SEM equipment and open the relevant software interface. Set the SEM acceleration voltage, magnification, scanning speed and other parameters on the software interface.
[0062] 3. Focus and Calibration
[0063] 1. Focus the sample by adjusting the objective lens and lens to make the image clear.
[0064] 2. Perform necessary calibration operations, such as adjusting the scanning speed and scanning mode of the electron beam, to ensure the accuracy and stability of the image.
[0065] IV. EDS analysis
[0066] 1. Select the test type: Select the EDS test type on the software interface, which usually includes point scanning (Point&ID), line scanning and surface scanning (Mapping).
[0067] 2. Scan image: Scan the sample to obtain an image according to the selected test type.
[0068] 3. EDS test: For point scan test, select the point or rectangular area to be tested, and the software will automatically perform spectrum test. For surface scan test, scan the image first, then select to collect distribution map data and start the test.
[0069] 4. Confirm the particle types in the sample by Auto ID or manual selection. Switch to the calculation component interface, edit the column and check the required component ratio (such as At%) to calculate the relative content of the particles.
[0070] The metal ion content was detected by inductively coupled plasma mass spectrometry (ICP-MS), which specifically includes the following steps:
[0071] 1. Sample pretreatment
[0072] 1. Sample digestion: Use acid digestion, microwave digestion, hot plate digestion and other methods to completely dissolve the sample while avoiding loss or contamination of the elements to be measured.
[0073] 2. Volume adjustment and dilution: The sample solution after digestion needs to be adjusted to an appropriate volume and necessary dilutions should be performed according to the concentration of the element to be measured to ensure that the measurement results are within the linear range of ICP-MS.
[0074] 3. Filtration and purification: To avoid the damage of suspended particles or impurities in the sample to the ICP-MS instrument, the sample solution after digestion needs to be filtered and purified through a filter membrane.
[0075] 2. Instrument Preparation
[0076] 1. Start-up preheating: Start the ICP-MS instrument and its supporting equipment (such as automatic sampler, gas source system, etc.), and preheat the instrument to a stable state.
[0077] 2. Instrument tuning: Use tuning fluid to tune the ICP-MS instrument and adjust various parameters of the instrument (such as RF power, plasma gas flow, sampling cone angle, etc.) to ensure that the instrument is in the best working state. During the tuning process, attention should be paid to performance indicators such as sensitivity, resolution, oxide and doubly charged ion ratio of the instrument.
[0078] 3. Sample determination
[0079] 1. Standard curve drawing: Use a series of standard solutions with known concentrations to draw a standard curve. The correlation coefficient of the standard curve should be above 0.99 to ensure the accuracy of the measurement results.
[0080] 2. Sample determination: Introduce the treated sample solution into the ICP-MS instrument for determination. According to the different mass-to-charge ratios of the elements to be determined, the instrument will automatically separate and detect the ion signal intensity of each element.
[0081] The test results are shown in Table 1.
[0082] Table 1 Particle content and metal ion content in the product used to produce electronic grade hydrofluoric acid in Example 1-2
[0083]
[0084] It can be seen from Table 1 that the hydrofluoric acid produced by the equipment and the inner wall of the pipeline after the vacuum plate lining is attached by the method of the present invention can reach the electronic grade and the E2 grade, which is of high quality.
[0085] The above experiments show that the high-strength attached vacuum plate lining technology adopted in the present invention is a special technology with the characteristics of corrosion resistance, wear resistance, high temperature resistance, chemical corrosion resistance, etc. It can effectively block the infiltration of metal ions and particulate matter into the inner wall of equipment and pipelines during the production process of wet electronic chemicals, greatly improve the purity of chemical products, and can meet the production requirements of G5-level wet electronic chemicals. It can creatively reduce the content of various metal ion impurities to below 5ppt, significantly improve economic benefits, and accelerate the production process of high-purity high-end chemicals.
[0086] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for attaching a vacuum lining, characterized in that: The specific steps include: (1) Performing ultra-fine composite grinding and polishing on the workpiece to be processed; (2) Apply glue to the wall surface of the workpiece to be processed and connect the non-woven fabric; (3) Apply glue on the surface of the non-woven fabric to connect the board lining material; (4) Ultrapure nitrogen is continuously introduced during ultrafine composite grinding and polishing, glue coating, and connecting non-woven fabrics and connecting plate lining materials, and high-pressure steam is continuously introduced during connecting non-woven fabrics and connecting plate lining materials; (5) A vacuum operation is performed between the inner wall of the workpiece to be processed and the plate lining material.
2. A method for attaching a vacuum lining according to claim 1, characterized in that: In step (1), the ultra-fine composite grinding and polishing includes at least one of ultrasonic grinding, magnetic grinding, chemical grinding and mechanical grinding.
3. A vacuum lining attachment method according to claim 2, characterized in that: The ultrasonic grinding is specifically as follows: placing the workpiece to be processed in an ultrasonic environment, wherein the ultrasonic wavelength λ is 0.02-2 cm.
4. A vacuum lining attachment method according to claim 2, characterized in that: The magnetic grinding is specifically as follows: high-performance grinding and polishing materials are filled into the workpiece to be processed, the workpiece is passed through by a fluid, and rotated at a certain speed while vibrating axially, and a strong DC magnetic field is applied in a plane direction perpendicular to the axis of the workpiece to be processed and the electric lines.
5. A vacuum lining attachment method according to claim 2, characterized in that: The chemical grinding specifically includes placing the workpiece to be processed in an electrolyte environment and passing an electric current to perform electrochemical processing.
6. A method for attaching a vacuum lining according to claim 1, characterized in that: In step (2) and step (3), the glue is at least one of acrylic acid, a modified copolymer emulsion of acrylic acid and vinyl acetate, and a hot melt adhesive film.
7. A vacuum lining attachment method according to claim 1, characterized in that: In step (2), the non-woven fabric is at least one of polypropylene, polyester, natural fiber and chemical fiber.
8. A vacuum lining attachment method according to claim 1, characterized in that: In step (3), the plate lining material is an alloy containing at least one of chromium, manganese and molybdenum, and is subjected to a quenching process, and the surface roughness Ra is less than 10 μm.
9. A vacuum lining attachment method according to claim 1, characterized in that: In step (4), the gauge pressure of the high-pressure steam is 10 to 200 kPa.
10. A vacuum lining attachment method according to claim 1, characterized in that: In step (5), the vacuum is evacuated to a gap absolute pressure of 30 to 98 kPa.
Citation Information
Patent Citations
Vacuum bonding method of anticorrosive fluoroplastic lining
CN102642305A
Litchi panel and cellular board composite technology
CN103264569A
Micro-fine structuralization surface finish machining method, medium and device
CN106584218A
Bi-metal composite abrasion-resistant pipe and preparation method thereof
CN106704720A
Manufacturing process of chemical storage tank
CN108620833A
Cited By
Rectification, separation and purification system and method for electronic-grade DFBP
CN122032126A
A distillation separation and purification system and method of electronic grade DFBP
CN122032126B