Polycarboxylic acid slump retaining mother liquor and preparation method thereof
The polycarboxylic acid slump-keeping mother liquor distributed through multiple groups is used to regulate the molecular weight of the polymer by acidic compounds and chain transfer agents, solving the problem of excessive settling time and water discharge of the slump-keeping agent, and achieving efficient maintenance of concrete slump and extension Effects of operational time.
Patent Information
- Application Number
- CN202411278450.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-09-12
AI Technical Summary
The existing slump retaining agents have problems such as long settling time, single hydroxyethyl acrylate exudates water during passing through, and the later loss of working performance is too fast.
Polycarboxylic acid slump-resistant mother liquor prepared using various components, including base material, liquid A and liquid B, and a redox system is composed of polyether large monomers, acrylic acid, small polyether monomers and carboxylic acid ester monomers. , acidic compounds are used to adjust the pH value, sodium hypophosphite and thiol chain transfer agent are used to regulate the molecular weight of the polymer, and improve the alkaline hydrolysis rate and water retention performance of the ester.
The polycarboxylic acid slump-keeping mother liquor is achieved to efficiently maintain the slump of concrete and extend the operable time, reduce water discharge and segregation, and improve the slump-keeping effect and adaptability.
Smart Images

Figure BDA0005040921590000091 
Figure BDA0005040921590000101
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of concrete admixtures, and in particular to a polycarboxylic acid collapse-preserving mother solution and a preparation method thereof. Background Art
[0002] Slump loss is a major problem in modern concrete construction. To improve this problem, existing scholars have developed some admixture products that can effectively inhibit slump loss. Among them, the main function of slump retaining agent is to enable the concrete mixture to maintain fluidity for a long time to meet the construction needs of modern concrete.
[0003] At present, in order to ensure that concrete can have good fluidity for a long time, the existing technology has improved the collapse-preventing agent. For example, the amount of retarding material is increased during the preparation process to solve the problem of collapse over time. However, this method has a slightly low cost-effectiveness and has hidden dangers such as excessively long setting time.
[0004] For example, methyl allyl polyoxyethylene ether (HPEG-2400) or isopentanol polyoxyethylene ether (TPEG2400) is polymerized with acrylic acid, hydroxyethyl acrylate, etc. to prepare a sustained-release polycarboxylic acid mother liquor, but problems such as water seepage after 1 to 1.5 hours and excessive loss after 2 hours are prone to occur.
[0005] Based on this, existing research and development of high-flowability collapse-preventing agents, such as the patent with publication number CN105399363B, which discloses a high-flowability concrete admixture and its preparation method, is compounded from a high-water-reducing polycarboxylate water-reducing agent mother liquor, a slow-release polycarboxylate water-reducing agent mother liquor, a thickener, a retarder and water. The raw materials of the high-water-reducing polycarboxylate water-reducing agent mother liquor include HPEG or TPEG; the raw materials of the slow-release polycarboxylate water-reducing agent mother liquor include polyoxyethylene methacrylate. This method can overcome the problem that existing admixtures are easy to separate and bleed when mixing high-flowability concrete, and the working performance loses quickly.
[0006] However, the above method separately prepares two reaction systems, namely, a high water-reducing polycarboxylate water-reducing agent mother liquor and a slow-release polycarboxylate water-reducing agent mother liquor, controls the compounding ratio of the two reaction systems, and also needs to control the mixing ratio of the two components in the slow-release polycarboxylate water-reducing agent mother liquor. The preparation process of this method is complicated, and the reaction cycle of the reaction system is long. Summary of the invention
[0007] In view of the shortcomings of the prior art, the present invention provides a polycarboxylic acid collapse-preventing mother solution and a preparation method thereof, so as to solve the problems of the existing collapse-preventing agent having a long setting time, single hydroxyethyl acrylate bleeding over time and a rapid loss of working performance in the later stage.
[0008] To achieve the above and related purposes, the present invention adopts the following technical solutions:
[0009] The first aspect of the present invention provides a polycarboxylic acid collapse-preserving mother solution, which is prepared from a plurality of components, wherein the plurality of components include a base material and a liquid A, wherein:
[0010] The base material includes a polyether macromonomer and a first pH regulator, wherein the polyether macromonomer is vinyl glycol ether polyoxyethylene ether, and the first pH regulator is selected from acidic compounds;
[0011] Liquid A includes acrylic acid, polyether small monomer and carboxylic acid ester monomer. The polyether small monomer is an aqueous solution of methacrylic acid polyoxyethylene ether, and the average molecular weight is 570-630.
[0012] Furthermore, the multiple components also include liquid B and a first chain transfer agent, and liquid B includes a second chain transfer agent. During preparation, the first chain transfer agent is first added to the base material, and then liquid B is added.
[0013] Furthermore, the mass ratio of the first pH adjuster to the polyether macromonomer is (0.3-0.8):100.
[0014] Furthermore, the first chain transfer agent is sodium hypophosphite, and the second chain transfer agent is a mercapto chain transfer agent.
[0015] Furthermore, the molar ratio of the polyether macromonomer, acrylic acid, polyether micromonomer, and carboxylate monomer is 1:(1-2.5):(0.2-1):(2-5).
[0016] Furthermore, the carboxylate monomer is selected from one or more of methyl acrylate, hydroxyethyl acrylate, and hydroxypropyl acrylate.
[0017] Furthermore, liquid B also includes a reducing agent and a second pH adjuster, and the second pH adjuster is selected from alkaline compounds.
[0018] Furthermore, the plurality of components also includes an aqueous solution of ferrous sulfate and an oxidizing agent.
[0019] The second aspect of the present invention provides a method for preparing a polycarboxylic acid collapse-preserving mother solution, comprising the following steps:
[0020] (1) preparing a base material: mixing water, a polyether macromonomer and a first pH adjuster to obtain a base material, wherein the polyether macromonomer is vinyl glycol ether polyoxyethylene ether, and the first pH adjuster is an acidic compound;
[0021] (2) preparing liquid A: mixing water, acrylic acid, a small polyether monomer and a carboxylic acid ester monomer to obtain liquid A, wherein the small polyether monomer is an aqueous solution of polyoxyethylene methacrylate and has an average molecular weight of 570 to 630;
[0022] (3) preparing liquid B: mixing water, a second pH adjusting agent, a reducing agent, and a second chain transfer agent to obtain liquid B;
[0023] (4) Add the first chain transfer agent, ferrous sulfate aqueous solution and oxidant to the base material in sequence, stir, add solution B and solution A dropwise to react, keep warm, add water to dilute, and obtain a polycarboxylic acid collapse mother solution.
[0024] Furthermore, the reaction temperature in step (4) is 10°C to 30°C.
[0025] The beneficial technical effects of the present invention are:
[0026] The invention utilizes polyether macromonomers, acrylic acid, polyether micromonomers and carboxylic acid ester monomers to form a novel redox system, and its free radical polymerization effect is better; the polyether micromonomer (aqueous solution of methacrylate polyoxyethylene ether) is used for side chain grafting modification, and the polyether micromonomer is introduced into the side chain to improve the alkaline hydrolysis rate of esters, so as to solve the problems of single hydroxyethyl acrylate such as water bleeding over time and excessive loss of working performance in the later stage.
[0027] The present invention selects an acidic compound as the first pH regulator to adjust the reaction pH, so as to increase the monomer dissolution rate, thereby shortening the reaction cycle and reducing the initial reaction rate, thereby increasing the proportion of effective polymer.
[0028] In the process of preparing the polycarboxylic acid slump-preserving mother solution, the chain transfer agent adopts a combination mode of adding sodium hypophosphite into the base material once and dripping a mercapto chain transfer agent, so as to better control the molecular weight of the polymer, thereby improving the water retention performance and slump retention ability of the slump-preserving mother solution.
[0029] The polycarboxylic acid collapse-preventing mother liquid of the invention has wider adaptability and better collapse-preventing effect; different branches are introduced into the side chain of the collapse-preventing mother liquid, which is hydrolyzed in the alkaline environment of concrete to generate the effective group carboxyl of the water reducer, thereby ensuring the continuous release ability of the product.
[0030] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. DETAILED DESCRIPTION
[0031] Unless otherwise defined, all technical and / or scientific terms used herein have the same meaning as the general understanding of a person of ordinary skill in the art to which the present invention belongs. It should be understood that certain features of the present invention (described in the context of separate embodiments for clarity) may also be provided in combination in a single embodiment. On the contrary, multiple features of the present invention (described in the context of a single embodiment for brevity) may also be provided separately or in any suitable combination or in any other described embodiment of the present invention when appropriate. Certain features described in the context of various embodiments will not be considered as essential features of those embodiments unless the embodiment is inoperable without those elements. The present invention is further described below by specific specific examples, but it should be noted that the specific process conditions and results described in the embodiments of the present invention are only used to illustrate the present invention, and the protection scope of the present invention cannot be limited thereto. All equivalent changes or modifications made according to the spirit and essence of the present invention should be included in the protection scope of the present invention.
[0032] The present invention provides a polycarboxylic acid collapse-preserving mother solution, which is prepared from a plurality of components, wherein the plurality of components include a base material and a liquid A, wherein:
[0033] The base material includes a polyether macromonomer and a first pH regulator, wherein the polyether macromonomer is vinyl glycol ether polyoxyethylene ether, and the first pH regulator is selected from acidic compounds;
[0034] Liquid A includes acrylic acid, polyether small monomer and carboxylic acid ester monomer. The polyether small monomer is an aqueous solution of methacrylic acid polyoxyethylene ether, and the average molecular weight is 570-630.
[0035] In some embodiments, the polyether macromonomer of the present application is preferably polyoxyethylene ether GPEG3000 produced by Jiangsu Sailbon. As part of the side chain, polyoxyethylene ether GPEG3000 participates in the synthesis of polycarboxylic acid collapse-retaining mother solution. This side chain structure gives the polycarboxylic acid collapse-retaining mother solution low dosage, high water reduction rate, high dispersibility, high collapse-retaining property and designable molecular structure characteristics.
[0036] In some embodiments, the polyether small monomer added in the present application is an 80% aqueous solution of polyoxyethylene methacrylate, which is PC-106. The role of the small monomer polyoxyethylene methacrylate in the collapse-preserving mother solution includes: improving the slump retention performance of concrete, extending the operability time of concrete, and preventing concrete shrinkage and cracking. There are almost no small molecular weight polyoxyethylene methacrylates in the existing collapse-preserving mother solutions. The present application selects low molecular weight polyoxyethylene methacrylate as a polyether small monomer, and uses it as a side chain branch to improve the alkaline hydrolysis rate of esters, which helps to maintain the dispersibility of cement, solve the shortcomings of single hydroxyethyl acrylate such as water bleeding over time and later loss, and further enhance the collapse-preserving performance of the collapse-preserving mother solution.
[0037] In some embodiments, the carboxylate monomer is selected from one or more of methyl acrylate, hydroxyethyl acrylate, and hydroxypropyl acrylate.
[0038] In some embodiments, the molar ratio of polyether macromonomer, acrylic acid, polyether micromonomer, and carboxylate monomer is 1: (1-2.5): (0.2-1): (2-5). The present application controls the molar ratio of each monomer component in the base material and the A liquid to adjust the acid-ether ratio in the collapse mother solution, so that the prepared collapse mother solution can provide better initial working performance and less time-dependent loss, and improve the dispersion performance and water retention performance of the collapse mother solution.
[0039] In some embodiments, the first pH adjuster of the present application is preferably acetic acid. Acetic acid is used to adjust the reaction pH value and increase the monomer dissolution rate, thereby shortening the reaction cycle and reducing the initial reaction rate, thereby increasing the proportion of effective polymer.
[0040] In some embodiments, the mass ratio of the first pH adjuster to the polyether macromonomer of the present application is (0.3-0.8):100.
[0041] In some embodiments, the multiple components further include liquid B and a first chain transfer agent, and liquid B includes a second chain transfer agent. During preparation, the first chain transfer agent is first added to the base material, and then liquid B is added.
[0042] In some embodiments, the first chain transfer agent is sodium hypophosphite, and the second chain transfer agent is a thiol chain transfer agent. The thiol chain transfer agent of the present application is selected from mercaptopropionic acid and / or mercaptoethanol.
[0043] In some embodiments, the present application uses polyether macromonomer, acrylic acid, polyether micromonomer, and carboxylic acid ester monomer as reaction units for free radical polymerization, and the mass ratio of sodium hypophosphite to reaction units is (0.5-2):100.
[0044] In some embodiments, the mass ratio of the thiol chain transfer agent to the reaction unit is (0.2-0.8):100.
[0045] In some embodiments, liquid B further comprises a reducing agent and a second pH adjusting agent, and the second pH adjusting agent is selected from alkaline compounds. The second pH adjusting agent of the present application is preferably sodium hydroxide. The reducing agent of the present application is selected from one or more of L-ascorbic acid, bleaching powder and imported E51.
[0046] In some embodiments, the plurality of components further comprises an oxidant. The oxidant of the present application is selected from hydrogen peroxide and / or sodium persulfate.
[0047] In some embodiments, the mass ratio of the reducing agent to the reaction unit is (0.1-0.4):100.
[0048] In some embodiments, the mass ratio of the oxidant to the polyether macromonomer is (0.5-1):100.
[0049] The present invention also provides a method for preparing a polycarboxylic acid collapse-preserving mother solution, comprising the following steps:
[0050] (1) preparing a base material: mixing water, a polyether macromonomer and a first pH adjuster to obtain a base material, wherein the polyether macromonomer is vinyl glycol ether polyoxyethylene ether, and the first pH adjuster is an acidic compound;
[0051] (2) preparing liquid A: mixing water, acrylic acid, a small polyether monomer and a carboxylic acid ester monomer to obtain liquid A, wherein the small polyether monomer is an aqueous solution of polyoxyethylene methacrylate and has an average molecular weight of 570 to 630;
[0052] (3) preparing liquid B: mixing water, a second pH adjusting agent, a reducing agent, and a second chain transfer agent to obtain liquid B;
[0053] (4) Add the first chain transfer agent, ferrous sulfate aqueous solution and oxidant to the base material in sequence, stir for 5 minutes, add liquid B and liquid A dropwise at a uniform rate to react, keep warm for 30 minutes to 60 minutes, add water to dilute to a concentration of 40%, and obtain a polycarboxylic acid collapse mother solution.
[0054] In some embodiments, the chain transfer agent of the present application adopts a combination mode of adding sodium hypophosphite into the base material once and adding a thiol chain transfer agent dropwise to better control the molecular weight of the polymer, thereby improving the water retention performance and slump retention ability of the slump-retaining mother solution.
[0055] In some embodiments, the water used herein is preferably deionized water.
[0056] In some embodiments, the mass concentration of the ferrous sulfate aqueous solution is 1%.
[0057] In some embodiments, the mass ratio of 1% ferrous sulfate aqueous solution to polyether macromonomer is (0.05-0.5):100.
[0058] In some embodiments, the dropwise addition time of solution B is 60 min to 80 min.
[0059] In some embodiments, the dropwise addition time of solution A is 50 min to 60 min.
[0060] In some embodiments, the temperature of the reaction system before dropwise addition is maintained at 10°C to 20°C, and the reaction temperature after dropwise addition is 10°C to 30°C, so as to control the speed of the chemical reaction, avoid unnecessary side reactions, avoid affecting the molecular structure and molecular weight distribution of the collapse-preserving mother solution, and improve the performance and stability of the collapse-preserving mother solution.
[0061] The present invention is described in detail below by specific examples. It should also be understood that the following examples are only used to specifically illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values exemplified below.
[0062] Example 1
[0063] (1) Preparation of base material: Add 3100 parts of deionized water to a reaction kettle equipped with a thermometer, a stirrer, a double dropping pipe and a reflux condenser, start stirring, add 3100 parts of polyoxyethylene ether GPEG3000 produced by Jiangsu Sailbon, add 15 parts of acetic acid, mix and dissolve to obtain a base material;
[0064] (2) preparing liquid A: 459 parts of deionized water, 108 parts of acrylic acid, 360 parts of polyether small monomer PC-106, 50 parts of methyl acrylate and 406 parts of hydroxyethyl acrylate were mixed to obtain liquid A;
[0065] (3) preparing liquid B: mixing 1000 parts of deionized water, 3 parts of solid sodium hydroxide, 8 parts of mercaptopropionic acid, 8 parts of mercaptoethanol and 11 parts of Rongbai to obtain liquid B;
[0066] (4) After the solid in the bottom material is dissolved and the temperature in the reactor is 10°C to 15°C, 20 parts of sodium hypophosphite, 5 parts of 1% ferrous sulfate aqueous solution, and 25 parts of 27.5% concentration of hydrogen peroxide are added in sequence. After stirring for 5 minutes, liquid B is added dropwise at a uniform speed for 60 minutes to 75 minutes and liquid A for 55 minutes to 60 minutes. After the addition is completed, the mixture is kept warm for 45 minutes to 60 minutes. 1290 parts of deionized water are added and mixed evenly to obtain a polycarboxylic acid collapse-preserving mother solution.
[0067] It should be noted that if the temperature exceeds 25°C during the reaction, cooling water should be added to ensure that the reaction temperature is below 30°C.
[0068] Example 2
[0069] The difference between this embodiment and embodiment 1 is that:
[0070] (1) Preparation of base material: Add 3100 parts of deionized water to a reaction kettle equipped with a thermometer, a stirrer, a double dropping pipe and a reflux condenser, start stirring, add 3100 parts of polyoxyethylene ether GPEG3000 produced by Jiangsu Sailbon, add 22 parts of acetic acid, mix and dissolve to obtain a base material.
[0071] Example 3
[0072] The difference between this embodiment and embodiment 1 is that:
[0073] (3) Preparation of Liquid B: Mix 1100 parts of deionized water, 3 parts of solid sodium hydroxide, 15 parts of mercaptopropionic acid, 15 parts of mercaptoethanol and 11 parts of Rongbai to obtain Liquid B.
[0074] Example 4
[0075] The difference between this embodiment and embodiment 1 is that:
[0076] (4) After the solid in the bottom material is dissolved, when the temperature in the reactor is 10°C to 15°C, 70 parts of sodium hypophosphite, 5 parts of 1% ferrous sulfate aqueous solution, and 25 parts of 27.5% concentration of hydrogen peroxide are added in sequence. After stirring for 5 minutes, liquid B is uniformly added for 60 minutes to 75 minutes and liquid A for 55 minutes to 60 minutes. After the addition is completed, the temperature is kept warm for 45 minutes to 60 minutes. 1320 parts of deionized water are added and mixed evenly to obtain a polycarboxylic acid collapse-preserving mother solution.
[0077] Comparative Example 1
[0078] The difference between this comparative example and Example 1 is:
[0079] (1) Preparation of base material: Add 3100 parts of deionized water to a reaction kettle equipped with a thermometer, a stirrer, a double dropping pipe and a reflux condenser, start stirring, add 3100 parts of polyoxyethylene ether GPEG3000, add 15 parts of acetic acid, mix and dissolve, and obtain a base material;
[0080] (2) Preparation of Liquid A: Mix 459 parts of deionized water, 108 parts of acrylic acid, 50 parts of hydroxypropyl acrylate and 406 parts of hydroxyethyl acrylate to obtain Liquid A.
[0081] Comparative Example 2
[0082] The difference between this comparative example and Example 1 is:
[0083] (1) Preparation of base material: Add 3100 parts of deionized water to a reaction kettle equipped with a thermometer, a stirrer, a double dropping pipe and a reflux condenser, start stirring, add 3100 parts of TPEG2400, add 15 parts of acetic acid, mix and dissolve, and obtain a base material;
[0084] (2) Preparation of Liquid A: Mix 459 parts of deionized water, 108 parts of acrylic acid and 406 parts of hydroxyethyl acrylate to obtain Liquid A.
[0085] Comparative Example 3
[0086] The difference between this comparative example and Example 1 is:
[0087] The average molecular weight of the polyether small monomer polyoxyethylene methacrylate ether is 1924.
[0088] Comparative Example 4
[0089] The difference between this comparative example and Example 1 is:
[0090] The base material does not contain acetic acid.
[0091] Comparative Example 5
[0092] The difference between this comparative example and Example 1 is:
[0093] No sodium hypophosphite is added in step (4).
[0094] Performance Testing
[0095] Collapse-preserving mother solution performance: The collapse-preserving mother solution performance of Example 1 and Comparative Examples 1 to 5 was tested, and the test results are shown in Table 1.
[0096] The test method is as follows: The fluidity of cement paste is tested according to the national standard GB / T8077-2012 "Test method for homogeneity of concrete admixtures". In each test sample, the amount of polycarboxylic acid slump-retaining solution in Example 1 and Comparative Examples 1 to 5 is 0.15% of the total mass of the adhesive, and W / C is 0.29. The test results are shown in Table 1.
[0097] The concrete test was conducted in accordance with the national standard GB 8076-2008 "Concrete Admixtures". The cement was Conch P·O 42.5, the sand was a mixture of fine sand with a fineness modulus of 1.8, machine-made sand with a fineness modulus of 3.2 and medium sand with a fineness modulus of 2.3, the average fineness modulus was 2.7, the gravel was continuously graded from 5mm to 31.5mm, and the admixture was 6 50% solid content examples 1 and comparative examples 1 to 5 respectively mixed with ordinary water-reducing polycarboxylic acid in a mass ratio of 5:5, and the admixture was 0.18% (solid) of the total mass of the cementitious material. The test was conducted according to the following mass mix ratio: cement: fly ash: sand: gravel: water: admixture = 280: 50: 800: 1080: 150: 0.594 (solid) (unit: kg / m 3 ), the test results are shown in Table 1.
[0098] The experimental data and analysis are as follows:
[0099] Table 1 Collapse-preserving mother liquor performance of Example 1 and Comparative Examples 1 to 5
[0100]
[0101]
[0102] As can be seen from Table 1, the fluidity of the cement paste of the polycarboxylic acid collapse-preserving mother solution prepared in Example 1 of the present application first increases and then remains within a period of 3 hours. The fluidity retention effect is obvious, and it has a good sustained-release effect, which can reduce the time loss of concrete.
[0103] The polycarboxylic acid slump-preserving concentrate prepared in Example 1 of the present application can maintain the slump and expansion of concrete for a long time, and can reduce bleeding and segregation, and reduce slump loss.
[0104] However, Comparative Examples 1 and 2 do not contain the polyether small monomer PC-106 of the present application, and the cement paste fluidity maintenance effect is poor, which has a negative impact on the working performance of the concrete, resulting in insufficient fluidity of the concrete during the construction process, large loss of concrete slump, and slight water seepage.
[0105] In Comparative Example 3, the molecular weight of the small polyether monomer is too high, and the side chain in the slump-preserving mother liquor is too large, which affects the alkaline hydrolysis rate of the ester, reduces the fluidity of the net paste, and causes a large loss in the slump of the concrete.
[0106] The base material of Comparative Example 4 does not contain acetic acid, and the proportion of effective polymer is low, which affects the effective dispersion and stabilization of the polymer on the cement particles, resulting in a decrease in the fluidity of the net paste, an accelerated loss of concrete slump, and the presence of water seepage.
[0107] In Comparative Example 5, the chain transfer agent did not adopt the combination mode of adding sodium hypophosphite into the base material once and adding the thiol chain transfer agent dropwise, resulting in the polymer molecular weight being too large, affecting the ability to maintain the slump of the concrete, and accelerating the slump loss. Although the initial fluidity of the pure paste in Comparative Example 5 was good, after a period of time, the ability to maintain the fluidity of the pure paste decreased significantly, and the effect of the slump-maintaining mother solution was poor.
[0108] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A polycarboxylic acid collapse-preserving mother solution, prepared from a plurality of components, wherein the plurality of components include a base material and a liquid A, characterized in that: The base material comprises a polyether macromonomer and a first pH adjuster, wherein the polyether macromonomer is vinyl glycol ether polyoxyethylene ether, and the first pH adjuster is selected from acidic compounds; The liquid A comprises acrylic acid, a small polyether monomer and a carboxylic acid ester monomer. The small polyether monomer is an aqueous solution of polyoxyethylene methacrylate, and has an average molecular weight of 570-630.
2. The polycarboxylic acid collapse-preserving mother solution according to claim 1, characterized in that: The multiple components further include liquid B and a first chain transfer agent, and the liquid B includes a second chain transfer agent. During preparation, the first chain transfer agent is first added to the base material, and then the liquid B is added.
3. The polycarboxylic acid collapse-preserving mother solution according to claim 1, characterized in that: The mass ratio of the first pH regulator to the polyether macromonomer is (0.3-0.8):
100.
4. The polycarboxylic acid collapse-preserving mother solution according to claim 2, characterized in that: The first chain transfer agent is sodium hypophosphite, and the second chain transfer agent is a thiol chain transfer agent.
5. The polycarboxylic acid collapse-preserving mother solution according to claim 1, characterized in that: The molar ratio of the polyether macromonomer, the acrylic acid, the polyether micromonomer and the carboxylate monomer is 1:(1-2.5):(0.2-1):(2-5).
6. The polycarboxylic acid collapse-preserving mother solution according to claim 1, characterized in that: The carboxylate monomer is selected from one or more of methyl acrylate, hydroxyethyl acrylate and hydroxypropyl acrylate.
7. The polycarboxylic acid collapse-preserving mother solution according to claim 2, characterized in that: The B solution further includes a reducing agent and a second pH adjusting agent, and the second pH adjusting agent is selected from alkaline compounds.
8. The polycarboxylic acid collapse-preserving mother solution according to claim 1, characterized in that: The plurality of components also includes an aqueous solution of ferrous sulfate and an oxidizing agent.
9. A method for preparing a polycarboxylic acid collapse-preserving mother solution, characterized in that: The following steps are involved: (1) preparing a base material: mixing water, a polyether macromonomer and a first pH adjuster to obtain a base material, wherein the polyether macromonomer is vinyl glycol ether polyoxyethylene ether, and the first pH adjuster is an acidic compound; (2) preparing liquid A: mixing water, acrylic acid, a small polyether monomer and a carboxylic acid ester monomer to obtain liquid A, wherein the small polyether monomer is an aqueous solution of polyoxyethylene methacrylate and has an average molecular weight of 570 to 630; (3) preparing liquid B: mixing water, a second pH adjusting agent, a reducing agent, and a second chain transfer agent to obtain liquid B; (4) adding a first chain transfer agent, an aqueous solution of ferrous sulfate and an oxidant to the base material in sequence, stirring, adding the liquid B and the liquid A dropwise to react, keeping the temperature, and adding water to dilute to obtain the polycarboxylic acid collapse-preserving mother solution.
10. The preparation method according to claim 9, characterized in that: The reaction temperature in step (4) is 10°C to 30°C.
Citation Information
Patent Citations
High-slump-resistance polycarboxylate water reducer
CN109734353A
High-slump-retaining mud-resistant polycarboxylate superplasticizer mother liquor as well as preparation method and application thereof
CN111116839A
Slow-release high-slump-loss-resistance polycarboxylic acid concrete water reducing agent and preparation method thereof
CN111607039A
High-water-reducing slump-retaining type polycarboxylate superplasticizer and preparation method and application thereof
CN111925489A
Premixed polyether for all-water spraying type rigid polyurethane and application thereof
CN116178655A