Application of oligomerization lignin in preparation of thermosetting phenolic resin

Oligoligin obtained by ultrasonic depolymerization reacts with formaldehyde and urea under alkaline conditions to prepare low-temperature curing, high-gluing strength lignin-based phenolic resin, which solves the toxicity problems of phenol and formaldehyde and wood in the prior art The problem of poor glue performance after carbon replacement has achieved environmentally friendly, low-pollution and high-performance phenolic resin adhesive.

CN118978652AActive Publication Date: 2024-11-19INST OF CHEM IND OF FOREST PROD CHINESE ACAD OF FORESTRY
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410929136.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-19
Estimated Expiration
2044-07-11

AI Technical Summary

Technical Problem

The existing thermosetting phenolic resins rely on highly toxic phenol and formaldehyde during the production process. They have high curing temperature and slow curing speed. They will release a large number of volatile organic compounds when used indoors, affecting air quality and human health. After lignin is directly replaced, they will be replaced by the lignin. Poor gluing performance and cannot meet national standards.

Method used

Ultrasonic depolymerization obtains oligolignin with narrow relative molecular mass distribution, partially replaces phenol, and combines formaldehyde and urea to prepare oligolignin-based phenolic resin under alkaline conditions to achieve low temperature curing and high glue strength.

Benefits of technology

Low-temperature curing, low formaldehyde emission and high glue strength are achieved, reducing the generation cost, and the formaldehyde emission is greatly reduced, and the curing temperature is reduced from 200℃ to 70℃, with better performance than undepolymerized and commercial phenolic resins.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978652A_ABST
    Figure CN118978652A_ABST
Patent Text Reader

Abstract

The invention relates to an application of oligomerization lignin in preparation of thermosetting phenolic resin. The preparation method comprises the following steps: replacing 55% of phenol with ultrasonically depolymerized oligomerization lignin, and preparing the thermosetting phenolic resin from formaldehyde and urea under an alkaline condition; the lignin is depolymerized at normal temperature in the depolymerization reaction, and the phenolic resin prepared by replacing 55% phenol with the oligomerization lignin with narrow relative molecular mass distribution (1t, 2) has the formaldehyde emission reduced to 0.07 mg / L from 0.147 mg / L, the gel temperature is also greatly reduced to 70 DEG C, and the wet shear strength is increased to 1.31 MPa from 1.17 MPa. The method has the advantages that the oligomerization lignin is obtained through the method which is mild in reaction condition, low in required reagent price, low in equipment requirement and good in repeatability, and the environment-friendly performance, the curing performance and the bonding performance of the phenolic resin adhesive prepared from the oligomerization lignin are all higher than those of a phenolic resin adhesive of a commercial formula.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the fields of utilization of agricultural and forestry wastes and preparation of phenolic resins, and in particular to application of oligomeric lignin in the preparation of thermosetting phenolic resins. Background Art

[0002] Phenolic resin (PF) is the first synthetic polymer with excellent water resistance and weather resistance, making it an ideal adhesive for outdoor wood-based panels. However, the production of phenolic resin relies on phenol and formaldehyde from the petrochemical industry, both of which are extremely toxic and non-renewable. In addition, there are some problems with thermosetting phenolic resins when used as adhesives, such as high curing temperature (the higher the curing temperature of the resin, the higher the energy consumption when preparing plywood, resulting in increased production costs) and slow curing speed, which have led to some restrictions on their application. Moreover, when used indoors, a large amount of volatile organic compounds (VOCs) will be released, which will have an adverse effect on indoor air quality and human health. Therefore, using low-toxic or non-toxic biomass raw materials to replace phenol and formaldehyde is a key strategy for developing more environmentally friendly and efficient adhesives.

[0003] Lignin is one of the most abundant natural aromatic polymers and a non-petroleum source of natural renewable aromatic compounds. It is an excellent substitute for phenol. This is because its phenylpropane units and abundant phenolic hydroxyl groups are similar in structure to phenol. However, when lignin is directly substituted for phenol to prepare phenolic resin, although the use of harmful substances such as phenol and waste utilization can be reduced, because the lignin structure contains more functional groups such as methoxyl groups and ether bonds, which increase steric hindrance and reduce its reactivity, the initial curing temperature of lignin-based phenolic resin is higher, the formaldehyde emission when used in wood adhesives remains high, and the bonding performance is also poor and difficult to meet national standards. Summary of the invention

[0004] Technical problem to be solved: The present invention provides an application of oligomeric lignin in the preparation of thermosetting phenolic resins, by directly obtaining oligomeric lignin with a narrow relative molecular mass distribution (<2) without the need for high temperature and expensive reagents, and then replacing most of the phenol to prepare a lignin-based phenolic resin with low pollution, low temperature curing, and strong bonding strength.

[0005] Technical solution: Application of oligomeric lignin in the preparation of thermosetting phenolic resin under the condition of partial replacement of phenol.

[0006] The application method is as follows: replacing 55% of phenol with oligomeric lignin obtained through ultrasonic depolymerization, and preparing thermosetting phenolic resin with formaldehyde and urea under alkaline conditions.

[0007] The specific steps are: adding phenol, water and sodium hydroxide solution into a reactor at a mass ratio of 1:1.25:1.25, adding lignin / oligomeric lignin and the first batch of formaldehyde solution at a replacement rate of 55% and a phenol-formaldehyde ratio of 0.4:1, and heating to start the reaction; after the reaction is completed, cooling down and adding the second batch of formaldehyde solution and sodium hydroxide solution, heating up to react; adding the third batch of formaldehyde solution, heating up to react; then adding urea, cooling down and discharging, to obtain lignin modified phenolic resin (LPF) / oligomeric lignin modified phenolic resin (DLPF).

[0008] Preferably, the mass ratio of the two additions of the sodium hydroxide solution is 3:2.

[0009] Preferably, the mass ratio of the three additions of the formaldehyde solution is 2:2:1.

[0010] Preferably, the mass fraction of the sodium hydroxide solution is 10%-30%.

[0011] Preferably, the lignin is enzymatic lignin, kraft lignin, alkali lignin or biomass butanol lignin.

[0012] The phenol, oligomeric lignin and formaldehyde are mixed and subjected to phenol-formaldehyde condensation under the action of a catalyst, sodium hydroxide. The reaction time of each phenol-formaldehyde condensation is 60-100 minutes, the reaction temperature is 90-95° C., and the amount of catalyst used is 0.75 times the mass of phenol.

[0013] Beneficial effects 1. There is no report on the application of oligomeric lignin obtained under normal temperature and ultrasonic conditions to the preparation of thermosetting phenolic resin. Oligomeric lignin has a higher hydroxyl content and reaction sites than raw material lignin (see Figure 1 ), and at the same time, the relative molecular mass distribution of lignin oligomers is narrow and uniform, which is helpful to improve the performance of lignin-based phenolic resins. 2. The entire lignin depolymerization process has mild conditions, simple operation, cheap and easy-to-obtain reagents, and obvious depolymerization effect, which has positive reference significance for the promotion of industrial production of lignin phenolic resins. 3. The substitution rate of oligomeric lignin in the synthesis of lignin-based phenolic resins is high, which can greatly reduce the production cost of lignin-based phenolic resins. 4. The formaldehyde emission in the oligomeric lignin phenolic resin synthesized from oligomeric lignin is extremely low, which can effectively improve the low pollution performance of lignin-based phenolic resin adhesives. 5. The curing performance of the oligomeric lignin phenolic resin synthesized by the method of the present invention is excellent, and curing can be completed at 70°C, which is much lower than the gel temperature of other lignin-based phenolic resins and industrial phenolic resins. 6. The oligomeric lignin phenolic resin synthesized by the method of the present invention has good properties such as bonding strength. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 This is the quantitative H-NMR spectrum of lignin oligomers.

[0015] After acetylation of oligomeric lignin, with p-nitrobenzaldehyde as the internal standard, the quantitative nuclear magnetic resonance hydrogen spectrum test was performed and the peak area was calculated to show that the hydroxyl content of oligomeric lignin was 36.9% higher than that of the undepolymerized lignin raw material. This is also the main reason why adding oligomeric lignin to phenolic resin can greatly improve its performance.

[0016] Figure 2 This is the temperature-dependent rheological test diagram of lignin-modified phenolic resin.

[0017] From this figure, it can be seen that adding lignin or oligomeric lignin to phenolic resin can reduce the curing temperature of phenolic resin. After adding oligomeric lignin, the curing temperature of phenolic resin is reduced from 200°C to 70°C, a decrease of 65%.

[0018] Figure 3 This is the relationship between the curing degree, curing rate and temperature of lignin-modified phenolic resin.

[0019] The curing rate and curing degree of lignin-modified phenolic resin can be calculated by first-order differential and second-order differential of the storage modulus in the variable temperature rheological test of lignin-modified phenolic resin. It can be clearly seen from the figure that the curing rate of phenolic resin can be increased by one order of magnitude after adding oligomeric lignin, which greatly improves the curing rate and curing degree. Figure 2 be consistent.

[0020] Figure 4 This is a comparison chart of the bonding properties and formaldehyde emission of lignin-modified phenolic resin.

[0021] Figure 5 This is a radar comparison chart of six key indicators of lignin-modified phenolic resin. DETAILED DESCRIPTION

[0022] The preparation method of oligomeric lignin is referred to CN114957704A, and the present invention is further described in conjunction with the examples:

[0023] Example 1

[0024] The raw material lignin was used to replace phenol to prepare lignin-based phenolic resin, and the lignin substitution rate (based on the total mass of lignin in lignin and phenol) was fixed at 55%, and the ratio of formaldehyde to phenol was 2.5. 2.0 kg of phenol, 2.5 kg of water and 1.5 kg of sodium hydroxide solution (mass fraction of 30%, 60% of the total amount) were added to a 20L reactor, 2.5 kg of raw material lignin and the first batch of formaldehyde solution (40% of the total amount) were added, and the temperature was raised to 90°C to start the reaction for 1 hour; the second batch of formaldehyde solution (40% of the total amount) and 1.0 kg of sodium hydroxide solution (40% of the total amount) were added, and the temperature was maintained at 90°C for 60 minutes; the third batch of formaldehyde solution (20% of the total amount) was added, and the temperature was lowered to 85°C for 30 minutes; urea was added, and the material was cooled to room temperature and discharged to obtain lignin-modified phenolic resin (LPF).

[0025] According to the analysis, the wet strength of lignin modified phenolic resin adhesive is 0.9MPa, its formaldehyde emission is 1.29mg / L, and the curing temperature is 180℃.

[0026] Example 2

[0027] Oligomeric lignin was used to replace phenol to prepare lignin-based phenolic resin, and the oligomeric lignin substitution rate (based on the total mass of oligomeric lignin in oligomeric lignin and phenol) was fixed at 55%, and the molar ratio of formaldehyde to phenol was 2.5. 2.0 kg of phenol, 2.5 kg of water and 1.5 kg of sodium hydroxide solution (mass fraction of 30%, 60% of the total amount) were added to a 20L reactor, 2.5 kg of oligomeric lignin and the first batch of formaldehyde solution (40% of the total amount) were added, and the temperature was raised to 90°C to start the reaction for 1 hour; the second batch of formaldehyde solution (40% of the total amount) and 1.0 kg of sodium hydroxide solution (40% of the total amount) were added, and the temperature was maintained at 90°C for 60 minutes; the third batch of formaldehyde solution (20% of the total amount) was added, and the temperature was lowered to 85°C for 30 minutes; urea was then added, and the material was cooled to room temperature and discharged to obtain oligomeric lignin modified phenolic resin (DLPF).

[0028] According to the analysis, the wet strength of the oligomeric lignin modified phenolic resin adhesive is 1.31MPa, the formaldehyde release is 0.07mg / L, and the gel temperature is 70℃.

[0029] Example 3

[0030] The raw material lignin was used to replace phenol to prepare lignin-based phenolic resin, and the lignin substitution rate (based on the total mass of lignin and phenol) was fixed at 33%, and the ratio of formaldehyde to phenol was 2.5. 2.0 kg of phenol, 2.5 kg of water and 1.5 kg of sodium hydroxide solution (mass fraction of 30%, 60% of the total amount) were added to a 20L reactor, 2.5 kg of raw material lignin and the first batch of formaldehyde solution (40% of the total amount) were added, and the temperature was raised to 90°C to start the reaction for 1 hour; the second batch of formaldehyde solution (40% of the total amount) and 1.0 kg of sodium hydroxide solution (40% of the total amount) were added, and the temperature was maintained at 90°C for 60 minutes; the third batch of formaldehyde solution (20% of the total amount) was added, and the temperature was lowered to 85°C for 30 minutes; urea was added, and the material was cooled to room temperature and discharged to obtain lignin-modified phenolic resin (LPF).

[0031] After analysis, the wet strength of the lignin-modified phenolic resin adhesive was 1.22 MPa and its formaldehyde emission was 0.25 mg / L.

[0032] Example 4

[0033] The raw material lignin was used to replace phenol to prepare lignin-based phenolic resin, and the lignin substitution rate (based on the total mass of lignin in lignin and phenol) was fixed at 43%, and the ratio of formaldehyde to phenol was 2.5. 2.0 kg of phenol, 2.5 kg of water and 1.5 kg of sodium hydroxide solution (mass fraction of 30%, 60% of the total amount) were added to a 20L reactor, 2.5 kg of raw material lignin and the first batch of formaldehyde solution (40% of the total amount) were added, and the temperature was raised to 90°C to start the reaction for 1 hour; the second batch of formaldehyde solution (40% of the total amount) and 1.0 kg of sodium hydroxide solution (40% of the total amount) were added, and the temperature was maintained at 90°C for 60 minutes; the third batch of formaldehyde solution (20% of the total amount) was added, and the temperature was lowered to 85°C for 30 minutes; urea was added, and the material was cooled to room temperature and discharged to obtain lignin-modified phenolic resin (LPF).

[0034] After analysis, the wet strength of the lignin-modified phenolic resin adhesive was 0.79 MPa and its formaldehyde emission was 0.08 mg / L.

[0035] Comparative Example 1

[0036] The raw material lignin and the lignin / oligomeric lignin obtained in Example 2 were used to replace phenol to prepare a lignin-based phenolic resin, with a fixed lignin / oligomeric lignin substitution rate (based on the total mass of lignin / oligomeric lignin in lignin / oligomeric lignin and phenol) of 55%, and the amount ratio of formaldehyde to phenol was 2.5. Add 2.0kg phenol, 2.5kg water and 1.5kg sodium hydroxide solution (30% by mass, 60% by total volume) to a 20L reactor, add 2.5kg raw lignin / oligomeric lignin and the first batch of formaldehyde solution (40% by total volume), heat to 90℃ and start reaction for 1h; add the second batch of formaldehyde solution (40% by total volume) and 1.0kg sodium hydroxide solution (40% by total volume), keep the temperature at 90℃ and react for 60min; add the third batch of formaldehyde solution (20% by total volume), cool to 85℃ and react for 30min; then add urea, cool to room temperature and discharge to obtain lignin modified phenolic resin (LPF) / oligomeric lignin modified phenolic resin (DLPF). For specific performance comparison, see Figure 4

[0037] Comparative Example 2

[0038] The oligomeric lignin obtained in Example 2 was used to replace phenol to prepare lignin-based phenolic resin (LPF) and compared with the phenolic resin (PF) prepared in the laboratory. The molar ratio of formaldehyde to phenol is 2.5. 4.4 kg of phenol, 2.5 kg of water and 1.5 kg of sodium hydroxide solution (mass fraction of 30%, 60% of the total amount) were added to a 20L reactor. The first batch of formaldehyde solution (40% of the total amount) was heated to 90°C to start the reaction for 1 hour; the second batch of formaldehyde solution (40% of the total amount) and 1.0 kg of sodium hydroxide solution (40% of the total amount) were added, and the temperature was maintained at 90°C for 60 minutes; the third batch of formaldehyde solution (20% of the total amount) was added, and the temperature was reduced to 85°C for 30 minutes; urea was added, cooled to room temperature and discharged to obtain the phenolic resin (PF) prepared in the laboratory. For specific performance comparison, see Figure 4 .

[0039] Comparative Example 3

[0040] The oligomeric lignin obtained in Example 2 was used to replace phenol to prepare lignin-based phenol-formaldehyde resin (LPF) and compared with the urea-formaldehyde resin (UF) prepared in the laboratory. For detailed performance comparison, see Figure 4

[0041] Comparative Example 4

[0042] The oligomeric lignin obtained in Example 2 was used to replace phenol to prepare the wood oligomeric lignin-based phenolic resin (DLPF) and compared with the laboratory-made urea-formaldehyde resin (PF). For detailed performance comparison, see Figure 4 .

[0043] In summary, the present invention applies lignin to the field of phenolic resins after ultrasonic-assisted depolymerization of lignin at room temperature to improve the reaction activity of lignin, and prepares green and efficient lignin-based phenolic resins. Compared with other lignin-based phenolic resins, the lignin depolymerization conditions of the present invention are mild, the equipment is simple, and it is green and environmentally friendly. The various properties of the oligomeric lignin-based phenolic resin prepared by the present invention are not only better than those of the undepolymerized lignin-based phenolic resin, but also stronger than those of commercial phenolic resins. Specifically, compared with commercial phenolic resins, the formaldehyde emission of the oligomeric lignin-based phenolic resin is reduced by about 50%, the gel temperature is also greatly reduced from 200°C to 70°C, and the wet shear strength is increased from 1.1MPa to 1.31MPa, thereby preparing an environmentally friendly, low-pollution and high-performance phenolic resin adhesive.

Claims

1. Application of oligomeric lignin in the preparation of thermosetting phenolic resin under the condition of partial replacement of phenol.

2. The use according to claim 1, characterized in that: Oligomeric lignin obtained by ultrasonic depolymerization replaced 55% of phenol and was reacted with formaldehyde and urea under alkaline conditions to prepare thermosetting phenolic resin.

3. The use according to claim 1, characterized in that: Phenol, water and sodium hydroxide solution are added into a reactor in a mass ratio of 1:1.25:1.25, lignin / oligomeric lignin and the first batch of formaldehyde solution are added at a replacement rate of 55% and a phenol-formaldehyde ratio of 0.4:1, and the temperature is raised to start the reaction; after the reaction is completed, the temperature is lowered and the second batch of formaldehyde solution and sodium hydroxide solution are added, and the temperature is raised to react; the third batch of formaldehyde solution is added, and the temperature is raised to react; urea is then added, the temperature is lowered and the material is discharged, so as to obtain lignin modified phenolic resin (LPF) / oligomeric lignin modified phenolic resin (DLPF).

4. The use according to claim 3, characterized in that: The mass ratio of the two additions of the sodium hydroxide solution is 3:

2.

5. The use according to claim 3, characterized in that: The mass ratio of the formaldehyde solution added three times is 2:2:

1.

6. The use according to claim 3, characterized in that: The mass fraction of the sodium hydroxide solution is 10%-30%.

7. The use according to claim 3, characterized in that: The lignin is enzymatic lignin, kraft lignin, alkali lignin or biomass butanol lignin.

8. The use according to claim 3, characterized in that: The phenol, oligomeric lignin and formaldehyde are mixed and subjected to phenol-formaldehyde condensation under the action of a catalyst, sodium hydroxide. The reaction time of each phenol-formaldehyde condensation is 60-100 min, the reaction temperature is 90-95° C., and the amount of the catalyst used is 0.75 times the mass of the phenol.

Citation Information

Patent Citations

  • Ultrasonic-assisted lignin oligomer preparation method

    CN114957704A

  • Method for preparing oxidized lignin phenolic resin adhesive

    CN106590488A

  • Production process of environment-friendly phenolic resin

    CN117757010A

  • Process for fungal modification of lignin and preparing wood adhesives with the modified lignin and wood composites made from such adhesives

    US20140163142A1