Non-metallic material for packaging light transmission equipment and preparation method of non-metallic material
By using a mixing system of natural rubber, styrene butadiene rubber and other components in the light transmission equipment, combining the coupling reaction of hydroxy silicone oil and silane coupling agent, the problems of light transmittance and cost in the prior art are solved, and the problem of high light transmission and cost is realized. High transparency and elasticity of optical transmission equipment packaging materials.
Patent Information
- Application Number
- CN202410910519.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-07-09
AI Technical Summary
In existing light transmission equipment, natural rubber/styrene butadiene rubber mixed system can easily lead to increased hardness and high cost when improving light transmittance. Especially when using vapor phase silica fillers, it is expensive and affects transparency.
The mixture system of natural rubber, styrene butadiene rubber, cycloolefin polymer, single-ended hydroxy silicone oil, fatty alcohol polyoxyethylene ether and silica filler is used to control the coupling reaction of hydroxy silicone oil and silane coupling agent. The spacing between silica particles reduces agglomeration phenomenon, and combines step-by-step refining technology to achieve a high light transmittance and high elasticity mixed rubber system.
The overall transparency is achieved above 90%, good mechanical properties are maintained, production costs are reduced, and the softness and elasticity of the rubber system are improved.
Smart Images

Figure BDA0004933442520000081 
Figure BDA0004933442520000091 
Figure BDA0004933442520000101
Abstract
Description
Technical Field
[0001] The present application relates to the field of optical signal transmission packaging materials, and in particular to a non-metallic material for packaging optical transmission equipment and a preparation method thereof. Background Art
[0002] The natural rubber / styrene-butadiene rubber mixed system is widely used in the preparation of internal rubber, which can play an important role in the fields of sealing, bonding, supporting, and rubber encapsulation protection. In optical communication or optical signal transmission equipment, the natural rubber / styrene-butadiene rubber-based blend can well protect the optical transmission medium. It has high softness, good bonding performance to each component, simple preparation, low cost, and is widely used.
[0003] SBR1500 is a commonly used raw material of styrene-butadiene rubber. After mixing with natural rubber, it can be vulcanized and kneaded to obtain a rubber system with good viscoelasticity. A series of fillers are usually added to the system, such as silica, calcium carbonate and other components. On the one hand, it can reduce the cost of rubber, and on the other hand, it also provides certain wear resistance, support strength and hardness.
[0004] Fillers in the system will greatly affect the light transmittance of the system, especially when the particle size is large. Usually, in order to improve the transparency of the rubber system, the filler needs to use an ultra-fine filler structure such as fumed silica, otherwise the light transmittance is difficult to exceed 80%. However, fumed silica is expensive and is prone to increase hardness after addition (especially when a silane coupling agent is added). Summary of the invention
[0005] The main purpose of this scheme is to provide a mixed rubber system with high light transmittance and high elasticity.
[0006] First, the present application provides a non-metallic material for packaging optical transmission equipment, which includes the following components in parts by mass:
[0007] Natural rubber 100 parts
[0008] Styrene butadiene rubber 50-70 parts
[0009] Cycloolefin polymer 15-30 parts
[0010] 5-10 parts of single-terminal hydroxyl silicone oil
[0011] 15-25 parts of silica filler
[0012] 1-2 parts of silane coupling agent;
[0013] 2-4 parts sulfur
[0014] 1-2 parts of accelerator
[0015] 3-5 parts of organic phosphorus flame retardant
[0016] Also included are fatty alcohol polyoxyethylene ethers, wherein the mass of the aliphatic polyoxyethylene ether is 0.3 to 0.5 times the mass of the cycloolefin polymer;
[0017] The particle size of the silica filler is not greater than 10 μm;
[0018] The styrene butadiene rubber is SBR-1500.
[0019] In the above scheme, nanoparticles with a silica particle size of nearly 1 μm can be accepted, and good transmittance can still be achieved, and the overall transmittance is not less than 60%. The reason is that in the above scheme, a coupling system with hydroxy silicone oil and silane coupling agent as the main body is added, so that the silica particles can be coupled with the hydroxy silicone oil to a certain extent. On the basis of the above, after the silica particles and the single-ended hydroxy silicone oil are coupled, the distance between the silica particles is far, so it is not easy to form a silica agglomeration system in the system that seriously affects the transparency. Therefore, even in the case of large silica particles, the scattering effect of light is still reduced, thereby maintaining good light transmittance.
[0020] In addition, cycloolefin polymers are added to the above system. Since cycloolefin polymers have a ring structure and are non-reactive, they will not adsorb silica. Instead, the barrier properties of their ring structure reduce the agglomeration of the silica / silicone oil system, further ensuring the transparency of the system. At the same time, cycloolefin polymers also improve the softness of the system, reduce the hardness to a certain extent, and improve the elasticity.
[0021] On the basis of the above, fatty alcohol polyoxyethylene ether is also added. Fatty alcohol polyoxyethylene ether has an excellent dispersion effect on silica in the system, and its fatty alcohol structure can better promote the compatibility of the silicone oil system with the natural rubber and styrene-butadiene rubber system. In the system based on natural rubber and styrene-butadiene rubber, the addition of fatty alcohol polyoxyethylene ether can effectively improve the dispersion performance of other hydrophilic components and further improve the uniformity of the system. In the system, the quality of fatty alcohol polyoxyethylene ether and cycloolefin polymer has a positive correlation. Since the ring structure in the cycloolefin polymer can improve its compatibility with the fatty alcohol end of fatty alcohol polyoxyethylene ether, and the softness of the polyoxyethylene ether chain is good, a more uniform, soft and high cohesive system can be formed in the above system, so that the overall strength and elasticity are maintained well.
[0022] Combining the above systems, the refractive index of the doping system formed by fatty alcohol polyoxyethylene ether and cycloolefin polymer is close to that of silica filler, and the overall transparency can reach about 90% without reducing its mechanical properties, so that the prepared rubber compound has good viscosity, elasticity and transparency.
[0023] In addition, the above system may also contain additives, such as antioxidants, anti-aging agents, etc., in a total amount not exceeding 10 parts by weight and having no effect on the transparency of the system.
[0024] Preferably, the cycloolefin polymer is a copolymer system of ethylene and norbornene, and further preferably, the cycloolefin polymer is TOPAS6013.
[0025] Cycloolefin polymers of the bornene system have better barrier properties and can better prevent the agglomeration of the silica system, thereby reducing light scattering in the system and improving light transmittance. Based on the above, after experiments, TOPAS6013 (purchased from Polyplastics or other companies) was used to obtain a plastic system with better overall strength, transparency and elasticity.
[0026] Preferably, the invention further comprises a tackifying resin, wherein the mass parts of the tackifying resin are 10 to 15 parts.
[0027] Tackifying resins can improve the viscosity, strength and cohesion of the system, so that it has good adhesion on different materials (such as PET plastic or similar rubber) while also having a certain improvement in internal strength.
[0028] Preferably, the mixture further comprises 3 to 5 parts by weight of white oil, wherein the white oil is No. 22 white oil, No. 32 white oil or No. 46 white oil.
[0029] White oil can play a lubricating role in the system. It has certain solvent properties. Therefore, adding white oil can make the components more evenly mixed during the mixing process, reduce the temperature required for mixing, and improve processing performance.
[0030] In the above scheme, No. 22 white oil, No. 32 white oil or No. 46 white oil is preferred. The above white oils have moderate viscosity. Continuing to use high-viscosity white oil will lead to poor mixing uniformity of the system, and hydroxy silicone oil and silica filler will be more easily precipitated in the system, which will lead to a decrease in the light transmittance of the system. The use of low-grade low-viscosity white oil will easily cause uneven mixing of materials, and non-polar systems (such as natural rubber and cycloolefin copolymers) cannot be evenly distributed in the system. In addition, it has good adhesion to the equipment during processing, and it is difficult to achieve smooth processing at a lower temperature, which will lead to an increase in the temperature required for processing.
[0031] Preferably, the viscosity of the single-end hydroxy silicone oil is 50-60 cst.
[0032] The silicone oil in the above viscosity range has just the right molecular chain length, which can ensure the appropriate particle spacing between the silica particles and achieve uniform system step-by-step. The use of short molecular chain and low viscosity hydroxy silicone oil will cause local agglomeration of silica, insufficient resistance between silica molecules, and easier agglomeration in an overall non-hydrophilic environment. The hydroxy silicone oil in the long molecular chain system is easy to cause agglomeration of the hydroxy silicone oil molecules themselves, and coupling on the silica surface will be more difficult to occur, which will also affect the transparency of the system.
[0033] Preferably, the fatty alcohol polyoxyethylene ether is Peregal O-10.
[0034] After experiments, it was found that when the fatty alcohol polyoxyethylene ether is Periga O-10, it has better dispersibility and uniformity for the system. After experiments, the obtained product has better strength and softness.
[0035] In addition, the present application also provides a method for preparing the above-mentioned optical transmission equipment packaging non-metallic material, comprising the following steps:
[0036] S1, kneading natural rubber, styrene-butadiene rubber, cycloolefin polymer, the first part of single-end hydroxyl silicone oil, fatty alcohol polyoxyethylene ether and the first part of silica filler at a kneading temperature of 100 to 120° C. for 20 to 40 seconds; preferably, white oil and tackifying resin may also be added in this step;
[0037] S2, adding the first silane coupling agent to the above system, and then adding the second part of the silica filler, heating to 140-145° C. for banburying for 10-15 seconds;
[0038] S3, adding the second part of silane coupling agent, the third part of silica filler and the second part of single-end hydroxy silicone oil to the above system, cooling to 130-140° C., and kneading for 1-2 minutes; in this step, the kneading time is preferably 75-90 seconds;
[0039] S4, adding sulfur and accelerator to the above system, maintaining 130-140°C, banburying for 40-60s, and discharging, the discharging temperature is 130-150°C;
[0040] The mass ratio of the first part of the single-end hydroxyl silicone oil to the second part of the single-end hydroxyl silicone oil is 1:0.5-2;
[0041] The mass ratio of the first part of the silane coupling agent to the second part of the silane coupling agent is 1:2-4;
[0042] The first part of the silica filler accounts for 30-40% of the mass of the silica filler, and the second part of the silica filler accounts for 20-30% of the mass of the silica filler.
[0043] In the above system, a system for reacting silica filler and epoxy coupling agent in steps is adopted. After experiments, it is found that if all silica, silicone oil and coupling agent are put into the system at one time, on the one hand, silica itself may agglomerate before the reaction, which will lead to color blocks and spots in the final product, affecting the color uniformity. On the other hand, after the coupling agent reacts quickly with the hydroxyl silicone oil, under the barrier of the organic phase system, the reaction temperature needs to be greatly increased to achieve a full reaction, which in turn affects the quality of the final rubber system.
[0044] Therefore, in the above scheme, the single-end hydroxy silicone oil and the silica filler are firstly pre-stepped and uniformly mixed in the system by a step-by-step reaction, and then part of the coupling agent is added to react, and the reaction is carried out twice, the first reaction is carried out at a higher temperature, and then the temperature is appropriately lowered, and the second reaction is carried out at a lower temperature. Overall, the two-step reaction is more conducive to the full and
[0045] Of course, another feasible solution is to fully react silica, hydroxy silicone oil and coupling agent outside the rubber system first, but this reaction step adds complexity to the processing process and is prone to introduce other impurities such as solvents. In particular, water may be introduced into the system, which will have a greater adverse effect on the rubber system.
[0046] In summary, in this scheme, a coupling structure is formed by coupling single-end hydroxy silicone oil and silica filler, and cycloolefin polymer and fatty alcohol polyoxyethylene ester are added to the system for dispersion, thereby obtaining a banburying rubber system with good transparency. At the same time, in the above process, the agglomeration of the silica filler is reduced by step-by-step banburying, so that the silica filler can still maintain good light transmittance when the particle size is large, thereby reducing the production cost. DETAILED DESCRIPTION
[0047] The preparation method of the non-metallic material for packaging optical transmission equipment described in this application is further described through the following specific implementation manner.
[0048] For the embodiments involved in this application, the performance is tested using the following experiments:
[0049] 1. Strength test: Refer to GB / T 528-2009 Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber to determine the tensile strength and elongation at break of the system.
[0050] 2. Rebound resilience test: Measured in accordance with ASTM-F36.
[0051] 3. Light transmittance test: refer to the national standard GB / T 2410-2008 Determination of light transmittance and haze of transparent plastics to measure the light transmittance of the sample. The sample thickness is 0.25mm.
[0052] In the following embodiments, experiments were conducted on commercially available SBR-1500 styrene-butadiene rubber, and the silica fillers used were all commercially available silica particles. In this solution, the silica filler used was silica with an average particle size of 8.5 μm, and was sieved to ensure that there were no particles with a particle size greater than 10 μm (the average particle size of 8.5 μm here is the particle size before sieving, but the proportion of large particle components after sieving is less than 1% of the total weight, so it has almost no effect on its average particle size).
[0053] In the following examples, the experimental data are obtained by small sample experiments, using experimental mixing equipment, and the single dosage does not exceed 1 kg. After the scale-up experiment was carried out on some experimental groups, the overall performance did not exceed the difference in measurement error. It can be determined that the experimental data in the following examples also have practical guiding significance after the scale-up experiment.
[0054] In Example 1, single-end hydroxyl silicone oil, double-end hydroxyl silicone oil and methyl silicone oil with different viscosities were used, and the amount of material added was kept uniform. In this embodiment, the amount of each material added was calculated in parts by mass as follows:
[0055]
[0056]
[0057] Among them, the styrene-butadiene rubber is SBR-1500, the cycloolefin polymer is TOPAS6013, the silane coupling agent is HK-550, the accelerator is the vulcanization accelerator CZ, and the organic phosphorus flame retardant is tri-o-cresyl phosphate. The silica filler is added in 25 parts by mass in this scheme, and the lower the silica mass dosage, the easier it is to obtain better transparency, so 25 parts by mass is used as the experimental benchmark in this scheme. In addition, in the above scheme, a small amount of antioxidants, anti-ultraviolet agents and other additives can also be added.
[0058] In this embodiment, the white oil used can be No. 22 white oil, No. 32 white oil or No. 46 white oil. White oil with a higher grade will increase the viscosity of the system, while white oil with a lower grade has poor solubility in the system, which will cause certain difficulties in the processing process. The tackifying resin is a commercially available terpene tackifying resin, the purpose of which is to improve the bonding performance of the system. The amount can be arbitrarily selected within 10 to 15 parts, and the effect on other mechanical properties and transparency is small. The aliphatic polyoxyethylene ether is Peregal O-10.
[0059] Regarding the ratio of styrene butadiene rubber to natural rubber, in most cases, the added amount of styrene butadiene rubber can be in the range of 50 to 70 parts by mass, which can have good softness and hardness.
[0060] The preparation method of this embodiment is as follows:
[0061] S1, mixing natural rubber, styrene-butadiene rubber, cycloolefin polymer, the first part of single-end hydroxy silicone oil, fatty alcohol polyoxyethylene ether, the first part of silica filler, white oil and tackifying resin at a mixing temperature of 120° C. for 20 seconds;
[0062] S2, adding the first silane coupling agent to the above system, heating to 140°C for banburying, and the banburying time is 15s;
[0063] S3, adding the second part of silane coupling agent, the second part of silica filler and the second part of single-ended hydroxyl silicone oil to the above system, cooling to 140°C, and mixing for 2 minutes;
[0064] S4. Add sulfur and accelerator to the above system, maintain the temperature at 140°C, mix for 60s, and discharge the material at a discharge temperature of 130-150°C.
[0065] Among them, the mass part of the first part of single-ended hydroxyl silicone oil is 5 parts, the mass part of the second part of single-ended hydroxyl silicone oil is 5 parts, the mass part of the first silane coupling agent is 0.67 parts, the mass part of the second part of the silane coupling agent is 1.33 parts, and the mass part of the first part of silica filler is 10 parts.
[0066] Table 1
[0067]
[0068] Through the experimental results in Example 1, it can be seen that in this scheme, only using single-end hydroxyl silicone oil has a better effect. Single-end hydroxyl silicone oil can ensure that a silicone oil molecular chain will not connect multiple silica fillers, and also ensure the good coupling performance between silicone oil and silica filler. At the same time, for the viscosity of silicone oil, it can be seen that when its viscosity is 50-60cts, the final product obtained has better light transmittance and elasticity. When double-end hydroxyl silicone oil is added to the system, regardless of the viscosity, it will have an adverse effect on light transmittance and easily harden the system as a whole. Ordinary silicone oil has little difference in light transmittance from the scheme without adding silicone oil, and will only slightly improve the resilience and mechanical strength of the system.
[0069] Example 2. In this scheme, a monohydroxy silicone oil with a viscosity of 53 cts is fixedly selected (i.e., the scheme of experimental groups 1-3), and different brands of cycloolefin polymers are used to study the specific roles of cycloolefin polymers and different cycloolefin polymers in the system. The specific experimental results are shown in Table 2.
[0070] Table 2
[0071]
[0072] Through the above experimental results, it can be seen that the selection of various cycloolefin polymers can improve the transparency of the system. This is not only because the cycloolefin polymer itself has high transparency, but also because the cycloolefin polymer is compatible with the silicone oil and silica particle composite system and its ability to reduce the generation of agglomeration in the rubber system. Under the arrangement of the cycloolefin molecular chain, the system greatly improves the transparency without significantly affecting the resilience. Among the various cycloolefin polymers, the selection of TOPAS6013 can have the best performance in terms of comprehensive mechanical properties, resilience and light transmittance.
[0073] Furthermore, on the basis of Example Nos. 1-3, the overall dosage of cycloolefin polymer and single-terminated hydroxyl silicone oil was adjusted as a whole. The specific experimental results are shown in Table 3.
[0074] Table 3
[0075]
[0076] It should be noted that during the quality adjustment of the single-ended hydroxyl silicone oil, the quality of the silane coupling agent used can be increased or decreased accordingly.
[0077] Through the above experiments, it can be seen that in this scheme, the mass proportion of silicone oil should be controlled at 5 to 10 parts. Too much silicone oil will lead to excessive dispersion of silica and silicone oil in the system, reduce the cohesion of the rubber system, and easily reduce the elongation at break and tensile strength. The cycloolefin polymer needs to be controlled under the condition of no more than 30 parts. Excessive use will lead to a decrease in the resilience of the system.
[0078] Furthermore, on the basis of experimental groups 1-3, different aliphatic polyoxyethylene ethers were selected, or other nonionic surfactants were used, and the overall mass was adjusted, and the experimental results shown in Table 4 were obtained.
[0079] Table 4
[0080]
[0081]
[0082] Through the above experimental results, it can be seen that compared with the Tween series of sorbitol non-ionic surfactants, fatty alcohol polyoxyethylene ethers represented by Peregrine have better effects as softeners and lubricants. The reason may be that the long-chain polyether structure can be better compatible with cycloolefin polymers and other rubber systems to improve the compatibility and uniformity of the overall components. After overall experiments, Peregrine O-10 has better mechanical properties and light transmittance.
[0083] Embodiment 5, the purpose of this embodiment is to select the importance of the step-by-step refining method, focusing on the adjustment of steps S1 to S3, as follows:
[0084] 5-1: Based on Example 1, step S2 is eliminated, the first silane coupling agent is directly added in step S1, and the kneading time of step S1 is adjusted to 35 seconds.
[0085] 5-2: Based on Example 1, step S2 is eliminated, and the first silane coupling agent is directly added to step S1, and the kneading time of step S1 is adjusted to 35 seconds and the temperature is adjusted to 140°C.
[0086] 5-3: Based on Example 1, step S2 is cancelled, and the first silane coupling agent is directly added in step S1, and the other steps remain unchanged.
[0087] 5-4: In step S1, all raw materials except sulfur and accelerator are directly added, and the temperature parameters of the specific mixing process remain unchanged.
[0088] 5-5: The temperature of step S1 is adjusted to 100°C and the time is adjusted to 40s;
[0089] 5-6: The temperature of step S2 is adjusted to 145°C and the time is adjusted to 10s;
[0090] 5-7: The temperature of step S2 is adjusted to 150°C and the time is adjusted to 7s;
[0091] 5-8: The temperature of step S3 is adjusted to 130°C and the time is adjusted to 1 min;
[0092] 5-9: The temperature of step S3 is adjusted to 120°C and the time is adjusted to 3 minutes;
[0093] 5-10: The temperature of step S3 is adjusted to 120°C;
[0094] 5-11: The temperature of step S3 is adjusted to 150°C and the time is adjusted to 1 minute;
[0095] 5-12: The temperature of step S3 is adjusted to 150° C. and the time is adjusted to 45 s;
[0096] 5-13: The mass parts of the first part of the single-end hydroxyl silicone oil are adjusted to 7.5 parts;
[0097] 5-14: The mass parts of the first part of the single-end hydroxyl silicone oil are adjusted to 2.5 parts;
[0098] 5-15: The mass fraction of the first part of the single-end hydroxyl silicone oil is adjusted to 1 part;
[0099] 5-16: The mass parts of the first part of the single-end hydroxyl silicone oil are adjusted to 2.5 parts, and the mass parts of the first part of the silica filler are adjusted to 7.5 parts;
[0100] 5-17: the mass part of the first part of the single-end hydroxy silicone oil is adjusted to 1 part, the mass part of the first part of the silica filler is adjusted to 5 parts, and the mass part of the first part of the silane coupling agent is adjusted to 0.4 parts;
[0101] 5-18: The mass fraction of the first part of the silane coupling agent is adjusted to 0.4 parts;
[0102] 5-19: The mass fraction of the first part of the silane coupling agent is adjusted to 0.2 parts;
[0103] 5-20: The mass fraction of the first part of the silane coupling agent is adjusted to 1 part;
[0104] 5-21; All silica fillers are added in step S1.
[0105] 5-22: The mass parts of the first part of silica filler are adjusted to 5 parts;
[0106] 5-23: The time of step S3 is adjusted to 75s;
[0107] 5-24: The time of step S3 is adjusted to 90s;
[0108] 5-25: The time of step S3 is adjusted to 105s.
[0109] It should be noted that in Example 5, the total amount of each material added remains unchanged. Taking experimental group 5-13 as an example, when the mass fraction of the first part of the single-ended hydroxyl silicone oil is adjusted to 7.5 parts, the mass fraction of the second part of the single-ended hydroxyl silicone oil is correspondingly adjusted to 2.5 parts.
[0110] The experimental results of Example 5 are shown in Table 5.
[0111] Table 5
[0112] serial number Tensile strength(mPa) Elongation at break (%) Resilience(%) Light transmittance (%) 1-3 10.6 567 59.2 91 5-1 10.2 558 57.4 85 5-2 9.9 530 57.8 85 5-3 9.4 544 54.0 82 5-4 9.0 557 54.4 76 5-5 10.3 558 59.5 90 5-6 10.4 556 59.5 91 5-7 10.0 553 57.3 87 5-8 10.0 588 57.1 91 5-9 9.8 567 58.0 86 5-10 9.8 566 58.6 84 5-11 10.3 545 56.0 87 5-12 10.4 551 55.4 88 5-13 10.5 572 59.0 91 5-14 10.7 576 59.6 90 5-15 10.0 570 59.2 87 5-16 10.5 562 59.5 92 5-17 10.1 561 57.4 86 5-18 10.3 558 60.4 91 5-19 9.9 545 59.5 88 5-20 10.4 570 57.2 87 5-21 10.5 553 54.1 84 5-22 9.7 544 57.0 83 5-23 10.8 579 59.0 93 5-24 11.0 569 59.3 93 5-25 10.5 564 58.9 91
[0113] It can be seen from the above steps that in this scheme, a step-by-step reaction method is required, and different amounts of single-end hydroxy silicone oil, silica filler and silane coupling agent are added in steps S1, S2 and S3 respectively. The main purpose of this step is to control the coupling rate of silica filler and silicone oil. Since other components in the system are almost inert compared to the silane coupling agent, the reaction will mainly occur in the silica filler and the silane coupling agent. On the whole, the reaction temperature in step S2 should be controlled within the range of 140 to 145°C as much as possible, and the time is preferably controlled within the range of 1 to 2 minutes. The optimal reaction time of step S3 is 75 to 90 seconds. Longer reaction times will cause the system to harden to a certain extent, and short reaction times will cause a certain decrease in the transparency of the product after discharge.
[0114] In the present embodiment, by comparing experimental groups 5-1 to 5-3, it can be seen that it is necessary to fully blend styrene-butadiene rubber and natural rubber with silicone oil before coupling to obtain a more uniform system. Experimental group 5-4 is a scheme in which all reactions are carried out at one time. The uniformity of the system in this step is difficult to guarantee, and silica itself is easy to agglomerate, so the system formed has the lowest transparency. In the remaining experimental groups, the parameters of each step are further adjusted. On the whole, the single-end hydroxy silicone oil mass parts added first can be 2.5 to 7.5 parts as a whole. Since it has good compatibility after being evenly dispersed in the system, it is not easy to agglomerate. Therefore, as long as it is not all added at one time, or too little is added in the early stage, it will not have a greater impact on the mechanical properties of the system, but silica filler and silane coupling agent will react faster after being added, so it needs to strictly control the amount added. Specifically, the mass parts of the filler added for the first time are preferably 7.5 to 10 parts by mass, and the silane coupling agent added for the first time is preferably 0.4 to 0.67 parts.
[0115] In addition, the reaction temperature of step S3 needs to be controlled at 130-140°C, and the banburying time needs to be controlled at 1-2min. On the whole, a better reaction effect can be obtained. When the reaction time is controlled at 75-90s, the obtained system has the best transparency (93%). After many experiments, this scheme can be confirmed as the best implementation method. In step S3, the system produces a second crosslinking, and the crosslinking system is also dispersed during the banburying process. If the reaction time is too short, it will lead to insufficient crosslinking or insufficient crosslinking of the system after crosslinking. The reaction time process is easy to cause the silica filler that has been fully dispersed in the system to precipitate, or produce partial chain breaks in the system, which will lead to a slight decrease in overall mechanical properties and transparency.
[0116] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A non-metallic material for packaging optical transmission equipment, characterized in that: The components include the following in parts by mass: Natural rubber 100 parts Styrene butadiene rubber 50-70 parts Cycloolefin polymer 15-30 parts 5-10 parts of single-terminal hydroxyl silicone oil Silica filler not more than 25 parts 1-2 parts of silane coupling agent; 2-4 parts sulfur 1-2 parts of accelerator 3-5 parts of organic phosphorus flame retardant Also included are fatty alcohol polyoxyethylene ethers, wherein the mass of the aliphatic polyoxyethylene ether is 0.3 to 0.5 times the mass of the cycloolefin polymer; The particle size of the silica filler is not greater than 10 μm; The styrene butadiene rubber is SBR-1500.
2. The optical transmission equipment packaging non-metallic material according to claim 1, characterized in that: The cycloolefin polymer is a copolymer system of ethylene and norbornene.
3. The optical transmission equipment packaging non-metallic material according to claim 2, characterized in that: The cycloolefin polymer is TOPAS6013.
4. The optical transmission equipment packaging non-metallic material according to claim 1, characterized in that: The invention also includes a tackifying resin, wherein the mass proportion of the tackifying resin is 10 to 15 parts.
5. The optical transmission equipment packaging non-metallic material according to claim 1, characterized in that: It also includes 3 to 5 parts by weight of white oil, wherein the white oil is selected from No. 22 white oil, No. 32 white oil or No. 46 white oil.
6. The optical transmission equipment packaging non-metallic material according to claim 1, characterized in that: The viscosity of the single-end hydroxy silicone oil is 50-60 cst.
7. The optical transmission equipment packaging non-metallic material according to claim 5, characterized in that: The fatty alcohol polyoxyethylene ether is Peregal O-10.
8. The method for preparing a non-metallic material for packaging optical transmission equipment according to any one of claims 1 to 6, characterized in that: The following steps are included S1, kneading natural rubber, styrene-butadiene rubber, cycloolefin polymer, the first part of single-end hydroxy silicone oil, fatty alcohol polyoxyethylene ether and the first part of silica filler at a kneading temperature of 100 to 120° C. for 20 to 40 seconds; S2, adding the first silane coupling agent to the above system, heating to 140-145° C. for banburying for 10-15 seconds; S3, adding the second part of silane coupling agent, the second part of silica filler and the second part of single-end hydroxy silicone oil to the above system, cooling to 130-140°C, and mixing for 1-2 minutes; S4, adding sulfur and accelerator to the above system, maintaining 130-140°C, banburying for 40-60s, and discharging, the discharging temperature is 130-150°C; The mass ratio of the first part of the single-end hydroxyl silicone oil to the second part of the single-end hydroxyl silicone oil is 1:0.5-2; The mass ratio of the first part of the silane coupling agent to the second part of the silane coupling agent is 1:2-4; The first part of the silica filler accounts for 30-40% of the mass of the silica filler.
9. The method for preparing a natural rubber / styrene-butadiene rubber mixed rubber according to claim 1, characterized in that: In step S1, white oil and tackifying resin are also added.
10. The method for preparing a non-metallic material for packaging optical transmission equipment according to claim 1, characterized in that: In step S3, the mixing time is 75 to 90 seconds.
Citation Information
Patent Citations
A curable transparent rubber composition, a cured transparent rubber composition made thereof, and manufacturing process for the same
CN108778659A
Preparation method of single-terminal hydroxyl silicone oil
CN112625242A
Flexible packaging material and preparation method thereof
CN113621163A
Polyvinyl alcohol film and preparation method of polaroid
CN116285179A
Modified rubber composite material and preparation method thereof
CN117126475A
Cited By
PO composite transfer printing film for out-of-mold transfer printing and preparation method of PO composite transfer printing film
CN120792277A