Pretreatment method for improving hydrophobicity of Fischer-Tropsch synthesis catalyst
Through calcination treatment and modification of hydrophobic agents with carbon chain length above C8, the problem of the reduction of activity of Fischer-Tropsch synthesis catalysts when improving hydrophobicity is solved, and the effect of high CO conversion and low CO2 selectivity is achieved, and oxides are avoided Use of encapsulation layers and poisons.
Patent Information
- Application Number
- CN202411230891.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-22
AI Technical Summary
When the existing Fischer-Tropsch synthesis catalyst improves hydrophobicity, the construction of an oxide encapsulation layer increases the surface OH content, hinders the contact between the reactants and the active center, and reduces the activity of the catalyst. The sulfur-containing and halogen-containing silanization reagents used at the same time are poisonous agents, resulting in the catalyst. Poisoning, activity decreases.
The Fischer-Tropsch synthesis catalyst after calcination is pre-activated, removes the surface adsorbed water, exposes the surface hydroxyl groups, and then mixes it with fatty acids or alkoxysilane hydrophobic agents with carbon chain length above C8 for hydrophobic modification, and combines washing. and dry to obtain a hydrophobic catalyst with a water droplet contact angle greater than 70°, avoiding the use of oxide encapsulation layer and poison.
It significantly reduces CO2 selectivity while maintaining high CO conversion, improves the hydrophobicity and activity of the catalyst, and avoids the defects of the introduction of oxide encapsulation layers and poisons.
Smart Images

Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the field of Fischer-Tropsch synthesis catalysts, and specifically relates to a pretreatment method for a Fischer-Tropsch synthesis catalyst, and more specifically relates to a pretreatment method for improving the hydrophobicity of a Fischer-Tropsch synthesis iron-based catalyst. Background Art
[0002] The Fischer-Tropsch synthesis reaction can convert carbon-containing resources such as coal, natural gas and biomass into liquid fuels and chemicals. It is a practical way to make up for the shortage of oil resources, ensure energy strategic security and achieve efficient and clean utilization of coal resources. After years of development, the indirect liquefaction technology with the Fischer-Tropsch synthesis reaction as the core has achieved industrial practice at the million-ton level per year. The outstanding problem facing indirect liquefaction technology is how to further reduce carbon emissions and improve energy conversion efficiency. Among them, the development of industrial catalysts with low CO2 selectivity is considered to be the key. Researchers have conducted a lot of useful explorations in this regard.
[0003] Patent application CN202010836695.2 discloses a catalyst and preparation method capable of inhibiting CO2 selectivity in the Fischer-Tropsch synthesis reaction. First, an iron-manganese oxide precursor is prepared, and then The method constructs a SiO2 shell on the surface of iron-manganese oxide, and finally silanizes the silica shell on the catalyst surface with chlorosiloxane to transform the hydrophilic surface into a hydrophobic surface. Reaction performance tests show that the CO2 selectivity of the optimal catalyst can be less than 10 mol%, but the corresponding CO conversion rate is less than 20%.
[0004] Based on this idea, patent application CN202210355783.X found that surface carbon modification of Fe / Cu / K / Si or Fe / Mn / K / Si catalysts can improve the hydrophobicity of the catalyst and inhibit the conversion of iron carbide to Fe3O4 during the reaction, thereby inhibiting CO2 selectivity. Among them, the CO2 selectivity of the optimal catalyst is 13.2mol%, and the CO conversion rate has increased (to 55.2%), but it is still at a low level. Then, the researchers used a variety of means to improve the hydrophobicity of the catalyst. For example, patent application CN202210515180.1 discloses a method of combining silanization treatment in two steps, which greatly improves the hydrophobicity of the FeMnCuSi precursor, so that the final CO2 selectivity can be reduced to about 1mol%, but the corresponding CO conversion rate is 32.5%. In addition, patent application CN202310117945.0 proposes a method of first preparing a hydrophobic carrier and then loading the active component. The method first prepares a hydroxyl-rich carrier, then uses fluorinated silane to hydrophobically modify the carrier, and finally loads the active phase iron species on the outer surface of the hydrophobic carrier. The performance evaluation of the prepared catalyst shows that the CO2 selectivity of the optimal catalyst can be reduced to about 10.89 mol%, and the CO conversion rate can be reduced to 25.96%.
[0005] In the current methods or processes for hydrophobic modification of Fischer-Tropsch synthesis catalysts, although CO2 selectivity has been significantly improved, in the process of constructing the hydrophobic layer, an oxide coating is often first constructed on the surface of the active component to increase the surface OH content, which is conducive to the subsequent introduction of a hydrophobic agent. However, the presence of the coating hinders the contact between the reactants and the active center, thereby reducing the activity of the catalyst. In addition, most of the hydrophobic agents currently used are silanization agents containing sulfur and / or halogens. Sulfur and halogens are considered to be poisons for Fischer-Tropsch synthesis catalysts. Their introduction will poison the catalyst, further causing a significant reduction in catalyst activity.
[0006] In view of this, there is an urgent need to develop an industrial catalyst hydrophobic treatment method that does not increase the OH content by constructing an oxide coating and does not use sulfur- and halogen-containing hydrophobic agents to reduce the CO2 selectivity of the catalyst. Summary of the invention
[0007] In order to solve the above-mentioned problems of the prior art, the present invention provides a method for preparing a Fischer-Tropsch synthesis catalyst which can effectively improve the hydrophobic effect of the catalyst and reduce the CO2 selectivity. The Fischer-Tropsch synthesis catalyst modified by this method can significantly reduce the CO2 selectivity in the Fischer-Tropsch synthesis reaction and maintain a high CO conversion rate.
[0008] In one aspect, the present invention provides a method for pretreating a Fischer-Tropsch synthesis catalyst, the method comprising:
[0009] (1) Providing a Fischer-Tropsch synthesis catalyst, which includes a calcination process;
[0010] (2) pre-activating the Fischer-Tropsch synthesis catalyst of step (1) to remove surface adsorbed water and fully expose the surface hydroxyl groups;
[0011] (3) immediately mixing the preactivated Fischer-Tropsch synthesis catalyst in step (2) with a hydrophobic agent solution and performing hydrophobic modification, and then washing and filtering with a washing solvent to obtain a hydrophobic Fischer-Tropsch synthesis catalyst precursor;
[0012] (4) Drying the hydrophobic Fischer-Tropsch synthesis catalyst precursor obtained in step (3) to obtain a hydrophobic Fischer-Tropsch synthesis catalyst.
[0013] In the present invention, the term "hydrophobic" means that the water drop contact angle of the Fischer-Tropsch synthesis catalyst is greater than 70°. For the purpose of the present invention, "hydrophobic" means a Fischer-Tropsch synthesis catalyst with higher hydrophobicity than the Fischer-Tropsch synthesis catalyst provided in step (1), specifically a Fischer-Tropsch synthesis catalyst with a larger water drop contact angle.
[0014] In the present invention, the term "hydrophobic Fischer-Tropsch synthesis catalyst" refers to a Fischer-Tropsch synthesis catalyst having a water drop contact angle greater than 70°.
[0015] In step (1), the Fischer-Tropsch synthesis catalyst prepared by a process including a calcination treatment is a supported or coprecipitated catalyst comprising an active metal, and an optional metal promoter and a structural promoter / carrier. In a specific embodiment, the active metal and the metal promoter include one or more of Fe, Mn, Cu, K, Ni, Co, Ca, Mg, Nb, Zr, B, Al, Ce, and La. In the Fischer-Tropsch synthesis catalyst provided in step (1), the active metal and the metal promoter are mainly present in the form of their oxides. In the present invention, the structural promoter or the carrier is selected from a SiO2 structural promoter or a silicon-containing carrier.
[0016] In the present invention, the Fischer-Tropsch synthesis catalyst is preferably a Fischer-Tropsch synthesis iron-based catalyst, that is, the active metal is Fe.
[0017] In the Fischer-Tropsch synthesis catalyst provided in step (1), the mass ratio of the active metal (calculated as metal element) to the total amount of metal in the metal additive is between (100:1) and (100:40), for example, (100:5) to (100:35), (100:10) to (100:30). For example, the mass ratio of Fe (calculated as Fe element) to the total amount of metal in the metal additive is between (100:1) and (100:40), for example, (100:5) to (100:35), (100:10) to (100:30).
[0018] In some embodiments, the Fischer-Tropsch synthesis catalyst comprises active metal Fe, and one or more metal promoters selected from Cu, Mn, Ca, K, La, Mg, Al, and Zr. In some embodiments, the Fischer-Tropsch synthesis catalyst comprises active metal Fe, and one or more metal promoters selected from Cu, Mn, Al, and K. In a specific embodiment, the Fischer-Tropsch synthesis catalyst comprises: Fe:Mn:Cu:Al:K is 100:15:3.5:4:6 (mass ratio).
[0019] In some embodiments, any form of Fischer-Tropsch synthesis catalyst may be subjected to hydrophobic modification pretreatment, including non-hydrophobically modified Fischer-Tropsch synthesis catalysts and hydrophobically modified Fischer-Tropsch synthesis catalysts. In some embodiments, any form of Fischer-Tropsch synthesis iron-based catalyst may be subjected to hydrophobic modification pretreatment, including non-hydrophobically modified Fischer-Tropsch synthesis iron-based catalysts and hydrophobically modified Fischer-Tropsch synthesis iron-based catalysts.
[0020] In a preferred embodiment, the method of the present invention is applicable to a Fischer-Tropsch synthesis catalyst that has not been hydrophobically modified, such as a Fischer-Tropsch synthesis iron-based catalyst.
[0021] In an embodiment of the present invention, in step (1), the Fischer-Tropsch synthesis catalyst may be a supported Fischer-Tropsch synthesis catalyst or a coprecipitated Fischer-Tropsch synthesis catalyst, including commercially available ones or prepared according to demand, for example, the preparation method can be obtained and adjusted by technicians according to actual needs. In the present invention, there are no special requirements for the specific surface area of the carrier, etc., and it can be used to prepare the Fischer-Tropsch synthesis catalyst. In some embodiments, the carrier can be selected from a carrier with a specific surface area greater than 100m 2 / g high specific surface area carrier, such as high specific surface area silica, or silicon-containing molecular sieve. For example, the carrier can be selected from dry silica gel, white carbon black, vapor deposited silica, ZSM-5 molecular sieve, diatomaceous earth.
[0022] As a preferred example, for supported catalysts, the precursors of active metals and promoter metals can be prepared by loading them on a carrier through impregnation, coprecipitation, water / solvothermal synthesis, chemical vapor deposition and / or atomic layer deposition.
[0023] For example, as an example of an impregnation method, the precursor of the active metal and the precursor of the auxiliary metal can be loaded on a carrier (the carrier can be selected from dry silica gel, white carbon black, vapor deposited silica, ZSM-5 molecular sieve, diatomaceous earth) by a co-impregnation or step-by-step impregnation method at any temperature, such as room temperature (such as 15°C-40°C). Among them, an exemplary co-impregnation method includes mixing the precursor of the active metal and the precursor of the auxiliary metal according to their composition ratio in the catalyst and dissolving them in a solvent to form an impregnation solution, and then impregnating the impregnation solution on the carrier. An exemplary step-by-step impregnation method is to dissolve the precursor of the active metal and the precursor of the auxiliary metal in a solvent to form a separate impregnation solution, and then impregnate the carrier step by step. Among them, the impregnation can be an equal volume impregnation or an excess impregnation. Equal volume impregnation means that the volume of the impregnation solution is equal to the pore volume of the carrier; excess impregnation means that the volume of the impregnation solution is greater than the pore volume of the carrier. For example, the active metal and the auxiliary metal may be loaded on the support by co-impregnating the support or a mixture thereof with an impregnation solution formed of a precursor of the active metal and a precursor of the auxiliary metal or by separate impregnation.
[0024] The solvent for forming the impregnation solution may be water, methanol, methylamine, dimethylamine, N,N-dimethylformamide, N-methylformamide, formamide, ethanol, ethylene glycol, diethyl ether, ethylamine, acetonitrile, acetamide, propanol, acetone, propionitrile, tetrahydrofuran, dioxane, butanol, pyridine, morpholine, quinoline, toluene, xylene, heptane or any mixture thereof, but is not limited thereto.
[0025] For example, as an example of a coprecipitation method, alternatively, the precursor of the active metal and the precursor of the auxiliary metal can be converted into a hydrated hydroxide and an oxide form by a coprecipitation method and deposited on a carrier (the carrier can be selected from dry silica gel, white carbon black, vapor-deposited silica, ZSM-5 molecular sieve, diatomaceous earth). Among them, the exemplary coprecipitation method includes mixing the precursor of the active metal and the precursor of the auxiliary metal according to their composition ratio in the catalyst and dissolving them in a solvent to form a mixed salt solution; mixing the mixed salt solution with the carrier powder according to the catalyst composition ratio and stirring to form a uniformly dispersed suspension; mixing the suspension with an alkaline precipitant solution, precipitating, standing, filtering, and washing to obtain a catalyst precursor. For example, the active metal and the auxiliary metal can be loaded on the carrier by forming a suspension with the mixed salt solution and the carrier or a mixture thereof, and then coprecipitating with an alkaline precipitant solution.
[0026] The alkaline precipitant solution can be an alkali metal hydroxide solution, such as an aqueous solution of sodium hydroxide and / or potassium hydroxide; it can also be an alkali metal carbonate or bicarbonate solution, such as an aqueous solution of sodium carbonate, sodium bicarbonate, potassium carbonate and / or potassium bicarbonate; it can also be an ammonia solution, an ammonium carbonate aqueous solution, an ammonium bicarbonate aqueous solution, preferably an ammonia solution.
[0027] Alternatively, the precursor of the active metal and the precursor of the auxiliary metal can be converted into metal, hydrated metal hydroxide, hydrated metal oxide, etc. by a water / solvothermal synthesis method and deposited on the support. For example, the active metal and the auxiliary metal can be loaded on the support by forming a mixed solution of the precursor of the active metal and the precursor of the auxiliary metal with the support or a mixture thereof in a solvent and performing water / solvothermal synthesis.
[0028] The solvent used to form the above mixed salt solution or alkali metal hydroxide solution or alkali metal carbonate solution or alkali metal bicarbonate solution and in the water / solvothermal synthesis method can be water, methanol, methylamine, dimethylamine, N,N-dimethylformamide, N-methylformamide, formamide, ethanol, ethylene glycol, ethylamine, acetonitrile, acetamide, propanol, propionitrile, tetrahydrofuran, dioxane, butanol, pyridine, morpholine, quinoline or any mixture thereof, but is not limited thereto.
[0029] Alternatively, the precursor of the active metal and the precursor of the auxiliary metal can be converted into metal, metal carbide, metal nitride, metal oxide, etc. by chemical vapor deposition and deposited on the support. For example, an organic metal compound containing the active metal and the auxiliary metal can be deposited in a high vacuum (10 -1 Pa-10 -6 The active metal and the auxiliary metal are deposited on the support or a mixture thereof by heating under conditions of 0.5 Pa (1 0.4 psi) or normal pressure (i.e., one atmosphere) and chemical vapor deposition.
[0030] Alternatively, the precursors of the active metal and the auxiliary metal can be converted into metals, metal carbides, metal nitrides, metal oxides, etc. by atomic layer deposition and deposited on the support. For example, the active metal and the auxiliary metal can be deposited on the support by atomic layer deposition in a high vacuum (10 -1 Pa-10 - 6 The gaseous compounds containing active metals and auxiliary metals and oxidants are alternately adsorbed in the Pa chamber, and the active metals and auxiliary metals are deposited on the carrier or their mixture by atomic layer deposition.
[0031] The precursor of the active metal is one or more selected from the following: ferric nitrate (preferably ferric nitrate nonahydrate), ferric chloride (preferably ferric chloride hexahydrate), ferrous chloride, ferrous sulfate, ferrous acetate, iron (III) acetylacetonate, carbonyl iron, ferrocene, but not limited thereto.
[0032] The precursor of the auxiliary metal is one or more selected from the following: copper nitrate, copper sulfate, copper chloride, manganese nitrate, manganese chloride, manganese acetate, manganese acetylacetonate, manganese carbonyl, potassium nitrate, potassium chloride, potassium hydroxide, potassium carbonate, potassium bicarbonate, potassium acetate, nickel acetate, nickel chloride, nickel nitrate, nickel sulfate, cobalt chloride, cobalt sulfate, cobalt nitrate, calcium nitrate, calcium chloride, calcium acetate, magnesium nitrate, magnesium chloride, magnesium acetate, niobium oxalate, niobium chloride, zirconium chloride, zirconium sulfate, zirconium nitrate, aluminum chloride, aluminum sulfate, aluminum nitrate, aluminum silicate, cerium chloride, cerium nitrate, lanthanum chloride, lanthanum nitrate, but not limited to these.
[0033] For the method of co-precipitation type Fischer-Tropsch synthesis catalyst, for example, the precursor of active metal and the precursor of auxiliary metal can be converted into hydrated hydroxide and oxide forms by co-precipitation method and deposited with structural additives. Among them, the exemplary co-precipitation method includes mixing the precursor of active metal and the precursor of auxiliary metal according to their composition ratio in the catalyst and dissolving them in a solvent to form a mixed salt solution; mixing and stirring the mixed salt solution with the structural additive in the form of sol according to the composition ratio of the catalyst to form a uniformly dispersed suspension; mixing the suspension with an alkaline precipitant solution, precipitating, standing, filtering, and washing to obtain a catalyst precursor. For example, a co-precipitation type catalyst can be obtained by forming a suspension with a mixed salt solution and a structural additive, and then co-precipitating with an alkaline precipitant solution.
[0034] The alkaline precipitant solution can be an alkali metal hydroxide solution, such as an aqueous solution of sodium hydroxide and / or potassium hydroxide; it can also be an alkali metal carbonate or bicarbonate solution, such as an aqueous solution of sodium carbonate, sodium bicarbonate, potassium carbonate and / or potassium bicarbonate; it can also be an ammonia solution, an ammonium carbonate aqueous solution, an ammonium bicarbonate aqueous solution, preferably an ammonia solution.
[0035] The Fischer-Tropsch synthesis catalyst in step (1) is one or both of a supported Fischer-Tropsch synthesis catalyst having a silicon-containing carrier or a coprecipitated Fischer-Tropsch synthesis catalyst containing a SiO2 structural aid. The mass ratio of Fe to the carrier (in terms of Si element) in the supported catalyst is between (10:100) and (50:100); the mass ratio of Fe to the structural aid (in terms of Si element) in the coprecipitated catalyst is between (100:1) and (100:50).
[0036] Furthermore, in step (1), the co-precipitated Fischer-Tropsch synthesis catalyst is prepared by co-precipitating the precursors of the active metal and the metal additive with the structural additive SiO2 under alkaline conditions, and filtering, washing, filter pressing, molding, and calcining to obtain a finished Fischer-Tropsch synthesis catalyst; the supported Fischer-Tropsch synthesis catalyst is prepared by impregnating the precursor solution of the active metal and the metal additive on a Si-containing carrier, and molding and calcining to obtain a finished Fischer-Tropsch synthesis catalyst that can be directly used.
[0037] In some embodiments, the Fischer-Tropsch synthesis iron-based catalyst comprises active metal Fe and a metal promoter, wherein the metal promoter is selected from one or more of Cu, Mn, K, Ni, Co, Ca, Mg, Nb, Zr, B, Al, Ce, and La.
[0038] In step (1), the calcination treatment is carried out at 450-700°C (e.g. 550-650°C, such as 500°C) for 1-12 hours (e.g. 2-10h, for example, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h or 10h).
[0039] In step (2), the pre-activation conditions include treating the Fischer-Tropsch synthesis catalyst for 1-12 hours (e.g., 2-10 hours, e.g., 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours or 10 hours) at 100°C-350°C (preferably 250°C-350°C, e.g., 250°C, 280°C, 300°C, 320°C or 350°C) under vacuum, air, nitrogen, argon or other inert gas atmosphere. The calcination in step (2) can at least remove adsorbed water, carbon dioxide, etc. on the catalyst surface.
[0040] In step (3), after the hydrophobic modification, the hydrophobic agent and the hydroxyl groups on the catalyst surface undergo dehydration condensation to form a hydrophobic structure of catalyst carrier / structural additive-oxygen-hydrophobic group. Therefore, without wishing to be bound by any theory, the hydrophobic modification method of the present invention can be used for all types of Fischer-Tropsch synthesis catalysts containing Si-based carriers or, and is not limited to the type of active metal or the type of additive metal.
[0041] In the present invention, the hydrophobic agent can be selected from fatty acids with a carbon chain length of C8 or more (such as stearic acid, etc.); and the general formula (RO) x R' 4-x Si alkoxysilane, wherein R is independently selected from C1-4 alkyl, R' is independently selected from C8-20 saturated or unsaturated, linear or branched alkyl, or 5-14 membered aromatic groups, and x is selected from an integer of 1-3. Among them, the fatty acid with a carbon chain length of more than C8 is preferably a C8-20 fatty acid, such as caprylic acid, capric acid, stearic acid, lauric acid, etc. Among them, R can be independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl; R' can be independently selected from octadecyl, n-octyl, phenyl, benzyl, phenethyl, etc.
[0042] In a specific embodiment, the hydrophobic agent can be selected from fatty acids with a carbon chain length of C8 or above (such as stearic acid, etc.), and alkoxysilanes such as dimethyldimethoxysilane, dimethoxydiphenylsilane, and n-octyltriethoxysilane.
[0043] In some embodiments, the organic solvent used to dissolve the hydrophobic agent can be selected from one or more solvents such as methanol, ethanol, ethylene glycol, propanol, N,N-dimethylformamide (DMF), benzene, toluene, xylene, cyclohexane, etc.
[0044] In some embodiments, the mass-to-volume ratio of the hydrophobic agent to the organic solvent in step (3) is 1:100 to 1:30, for example, 1:100, 1:90, 1:80, 1:70, 1:60, 1:50, 1:40 or 1:30.
[0045] In a specific embodiment, the mass ratio of the hydrophobic agent added in step (3) to the catalyst is (0.05-0.5):1, for example, 0.05:1, 0.1:1, 0.15:1, 0.2:1, 0.25:1, 0.3:1, 0.35:1, 0.4:1, 0.45:1 or 0.5:1.
[0046] In a specific embodiment, the temperature of the hydrophobic modification in step (3) is 80°C-160°C (e.g., 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C or 160°C), and the time is 1-12 hours (e.g., 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h or 12h).
[0047] In a preferred embodiment, during the hydrophobic modification process in step (3), ultrasonic treatment, condensation reflux or stirring of the solvent are simultaneously performed to ensure sufficient reaction and the solvent is not evaporated. In some embodiments, the conditions of the ultrasonic treatment are: ultrasonic power 300-1000W (e.g., 500W), frequency above 20KHz (e.g., 40KHz), and ultrasonic time 1-5h.
[0048] Before step (3), the preactivated catalyst obtained in step (2) is cooled to room temperature. In the present invention, "room temperature" refers to ambient temperature, such as 15°C-40°C.
[0049] After the hydrophobic modification in step (3) is completed, the catalyst is washed and filtered using a solvent corresponding to the hydrophobic agent to remove the unbound hydrophobic agent to obtain a hydrophobic Fischer-Tropsch synthesis catalyst precursor. The washing solvent may be one or more of cyclohexane, toluene, xylene, and ethanol.
[0050] The drying conditions in step (4) are 80-200° C. (preferably 100-200° C.) for 2-12 hours (e.g., 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, or 12h) in air or nitrogen atmosphere.
[0051] In one aspect, the present invention also relates to a hydrophobic Fischer-Tropsch synthesis catalyst prepared by the above method.
[0052] The present disclosure also relates to the use of the above catalyst for catalyzing synthesis gas in a Fischer-Tropsch synthesis reaction to prepare hydrocarbon compounds. Alternatively, the present disclosure also relates to a Fischer-Tropsch synthesis reaction method, wherein the above Fischer-Tropsch synthesis catalyst is used to catalyze synthesis gas to carry out a Fischer-Tropsch synthesis reaction to prepare hydrocarbon compounds.
[0053] As a preferred example, before the hydrophobic catalyst of the present invention is applied to the Fischer-Tropsch synthesis reaction, the catalyst is pre-activated in a reducing atmosphere. The reducing atmosphere may be a pure hydrogen atmosphere, a CO atmosphere, a synthesis gas atmosphere, an ammonia atmosphere, a diluted hydrogen atmosphere, a diluted CO atmosphere, a diluted synthesis gas atmosphere, or a diluted ammonia atmosphere. The volume ratio of H2 to CO in the synthesis gas is 0.01:1 to 1000:1. For example, when reacting in a fixed bed, the conditions for the activation pretreatment are: a temperature of 230-450°C, H2 / CO in the fresh gas = 1-50 (molar ratio), and a space velocity of 1000-10000h -1 , the circulation ratio is 0-10, the pressure is 0.1-5.5MPa, and the time is 10-60h. The reaction conditions of Fischer-Tropsch synthesis are: temperature is 250-350℃, H2 / CO in fresh gas is 1-10 (molar ratio), and the space velocity is 3000-30000h -1 , the circulation ratio is 1-5, and the pressure is 0.1-5.5MPa.
[0054] For example, when the reaction is carried out in a slurry bed, the conditions for activation pretreatment are: temperature of 230-300°C, H2 / CO in the fresh gas = 1-50 (molar ratio), and space velocity of 3000-10000h -1 , the circulation ratio is 0-10, the pressure is 0.1-5.5MPa, and the time is 10-60h. The reaction conditions of Fischer-Tropsch synthesis are: temperature is 250-300℃, H2 / CO in fresh gas is 1-10 (molar ratio), and the space velocity is 3000-30000h -1 , the circulation ratio is 1-5, and the pressure is 0.1-5.5MPa.
[0055] The present invention has the following beneficial effects:
[0056] The preparation method of the present invention directly uses the finished catalyst after calcination, and improves the OH content on the catalyst surface by optimizing the pre-activation. The surface OH content can be increased without constructing an oxide covering layer (and thus without covering the active sites). Combined with the use of a sulfur-free and halogen-free hydrophobic agent, the technical goal of ultimately improving the hydrophobicity of the catalyst and thereby reducing the CO2 selectivity without losing the CO conversion rate of the catalyst can be achieved. DETAILED DESCRIPTION
[0057] The specific embodiments of the present invention are described in detail below. The specific embodiments described here are only used to illustrate and explain the present invention, but are not used to limit the present invention.
[0058] The present invention is further described below by way of examples, but the present invention is not limited thereto.
[0059] Example
[0060] Unless otherwise specified, the reagents, materials and devices involved in the following examples were purchased from conventional suppliers in the art.
[0061] Preparation Example 1
[0062] Weigh 4406.28 grams of ferric nitrate nonahydrate, 586.38 grams of manganese nitrate aqueous solution (concentration 50wt%), 80.64 grams of copper nitrate trihydrate, and 338.73 grams of aluminum nitrate nonahydrate, add 3000 grams of deionized water to fully dissolve the above nitrates, and prepare a mixed nitrate solution for use, then add 514.29 grams of silica sol with a SiO2 mass content of 30%, stir well, and the composition is: Fe: Mn: Cu: Al: Si = 100: 15: 3.5: 4: 12 (mass ratio), and heat to 70°C; take 10.00wt% ammonia The aqueous solution was preheated to 40°C, and continuously co-precipitated at 80°C and pH 6.5 under stirring; aged for 1 hour after precipitation, washed until the ammonium nitrate content in the slurry was less than 0.1wt%, and filtered to obtain a filter cake; 600g of deionized water and 92.64g of potassium bicarbonate were added to the filter cake so that the mass ratio of iron to K was 100:6.0; after sufficient slurrying; the obtained slurry was spray-dried, and the inlet air temperature was controlled at 400°C and the outlet air temperature was controlled at 105°C; the spray-dried powder was roasted at 500°C for 3 hours to obtain a finished catalyst, which was recorded as catalyst-1.
[0063] Preparation Example 2
[0064] Hydrophobic treatment of the catalyst: 20 g of catalyst-1 was added to a cyclohexane solution of dimethyldimethoxysilane (wherein 2 g of dimethyldimethoxysilane was dissolved in 200 mL of cyclohexane), heated to 80°C and stirred for 2 hours under cooling and reflux conditions; washed and filtered 3 times with anhydrous ethanol, and dried at 120°C in an air atmosphere for 5 hours to obtain a finished catalyst. This catalyst was recorded as catalyst-2.
[0065] Example 1
[0066] Pre-activation of the catalyst: 20 g of catalyst-1 was calcined at 300° C. for 3 hours in a vacuum-evacuated tube furnace.
[0067] Hydrophobic modification of the catalyst: add an anhydrous ethanol solution of stearic acid (wherein 4 g of stearic acid is dissolved in 200 mL of anhydrous ethanol) to the pre-activated catalyst cooled to room temperature, heat to 100°C under cooling and reflux conditions, and stir for 3 hours; then wash and filter 3 times with cyclohexane to obtain a hydrophobic Fischer-Tropsch synthesis catalyst precursor.
[0068] Drying: The obtained hydrophobic Fischer-Tropsch synthesis catalyst precursor was dried at 120° C. for 6 hours under a nitrogen atmosphere to obtain a finished hydrophobic Fischer-Tropsch synthesis catalyst.
[0069] This catalyst is referred to as Catalyst A.
[0070] Example 2
[0071] Pre-activation of the catalyst: 20 g of catalyst-1 was calcined at 280° C. for 5 hours under a nitrogen atmosphere.
[0072] Hydrophobic modification of the catalyst: Add a toluene solution of dimethoxydiphenylsilane (wherein 8 g of dimethoxydiphenylsilane is dissolved in 400 mL of toluene) to the pre-activated catalyst cooled to room temperature, heat to 140°C under cooling and reflux conditions, and simultaneously perform ultrasonic treatment (ultrasonic power 500 W, frequency 40 kHz) for 2 hours; then wash and filter 3 times with toluene to obtain a hydrophobic Fischer-Tropsch synthesis catalyst precursor.
[0073] Drying: The obtained hydrophobic Fischer-Tropsch synthesis catalyst precursor was dried at 160° C. for 5 hours in an air atmosphere to obtain a finished hydrophobic Fischer-Tropsch synthesis catalyst.
[0074] This catalyst is referred to as catalyst B.
[0075] Example 3
[0076] Pre-activation of the catalyst: 20 g of catalyst-1 was calcined at 320° C. for 5 hours in an air atmosphere.
[0077] Hydrophobic modification of the catalyst: add a xylene solution of n-octyltriethoxysilane (wherein 6 g of n-octyltriethoxysilane is dissolved in 300 mL of xylene) to the pre-activated catalyst cooled to room temperature, heat to 150°C under cooling and reflux conditions, and perform ultrasonic treatment (ultrasonic power 500 W, frequency 40 kHz) for 3 hours; then wash and filter 3 times with xylene to obtain a hydrophobic Fischer-Tropsch synthesis catalyst precursor.
[0078] Drying: The obtained hydrophobic Fischer-Tropsch synthesis catalyst precursor was dried at 170° C. for 4 hours in an air atmosphere to obtain a finished hydrophobic Fischer-Tropsch synthesis catalyst.
[0079] This catalyst is referred to as Catalyst C.
[0080] Example 4
[0081] Pre-activation of the catalyst: 20 g of catalyst-1 was calcined at 300° C. for 3 hours under an argon atmosphere.
[0082] Hydrophobic modification of the catalyst: add a xylene solution of octadecyltrimethoxysilane (wherein 10 g of octadecyltrimethoxysilane is dissolved in 400 mL of xylene) to the pre-activated catalyst cooled to room temperature, heat to 130°C under cooling and reflux conditions, and stir for 12 hours; then wash and filter three times with xylene to obtain a hydrophobic Fischer-Tropsch synthesis catalyst precursor.
[0083] Drying: The obtained hydrophobic Fischer-Tropsch synthesis catalyst precursor was dried at 180° C. for 10 hours under a nitrogen atmosphere to obtain a finished hydrophobic Fischer-Tropsch synthesis catalyst.
[0084] This catalyst was recorded as Catalyst D.
[0085] Catalyst performance evaluation
[0086] The hydrophobicity of the catalyst was evaluated by recording the water drop contact angle in a water drop experiment.
[0087] All catalyst performance evaluations were conducted in a 2000 mL continuous stirred slurry bed reactor. Before the Fischer-Tropsch synthesis performance evaluation, the catalyst was activated and pretreated. The activation and pretreatment conditions were: temperature 260°C, H2 / CO in fresh gas = 1.9 (molar ratio), space velocity 9000 h -1 , the circulation ratio is 8, the pressure is 3.0MPa, and the time is 30h.
[0088] The reaction conditions of the Fischer-Tropsch synthesis reaction process for performance evaluation are shown in Table 1 below, where the fresh synthesis gas H2 / CO is 1.7 (molar ratio).
[0089]
Claims
1. A pretreatment method for a Fischer-Tropsch synthesis catalyst, the method comprising: (1) Providing a Fischer-Tropsch synthesis catalyst, which includes a calcination process; (2) pre-activating the Fischer-Tropsch synthesis catalyst of step (1) to remove surface adsorbed water and fully expose the surface hydroxyl groups; (3) immediately mixing the preactivated Fischer-Tropsch synthesis catalyst in step (2) with a hydrophobic agent solution and performing hydrophobic modification, and then washing and filtering with a washing solvent to obtain a hydrophobic Fischer-Tropsch synthesis catalyst precursor; (4) Drying the hydrophobic Fischer-Tropsch synthesis catalyst precursor obtained in step (3) to obtain a hydrophobic Fischer-Tropsch synthesis catalyst.
2. The method according to claim 1, wherein: The Fischer-Tropsch synthesis catalyst in step (1) comprises an active metal, a metal promoter and a structural promoter / carrier; Preferably, the active metal is Fe, the metal additive is selected from one or more of Mn, Cu, K, Ni, Co, Ca, Mg, Nb, Zr, B, Al, Ce, and La, and the structural additive or carrier is selected from SiO2 structural additive or silicon-containing carrier; More preferably, the mass ratio of the active metal to the total amount of metal elements in the metal additive is between (100:1)-(100:40), preferably (100:5)-(100:35).
3. The method according to claim 1 or 2, wherein: The Fischer-Tropsch synthesis catalyst described in step (1) is a supported Fischer-Tropsch synthesis catalyst or a coprecipitated Fischer-Tropsch synthesis catalyst; Preferably, in the supported Fischer-Tropsch synthesis catalyst, the mass ratio of active metal Fe to the carrier is between (10:100) and (50:100), wherein the carrier is calculated as Si element; in the co-precipitated Fischer-Tropsch synthesis catalyst, the mass ratio of active metal Fe to the structural additive is between (100:1) and (100:50), wherein the structural additive is calculated as Si element.
4. The method according to any one of claims 1 to 3, wherein: In step (1), the calcination treatment is carried out at 450°C-700°C, preferably 550-650°C, for 1-12 hours.
5. The method according to any one of claims 1 to 4, wherein: In step (2), the pre-activation conditions include treating the Fischer-Tropsch synthesis catalyst for 1-12 hours at 100°C-350°C, preferably 250°C-350°C, under vacuum, air, nitrogen, argon or other inert gas atmosphere.
6. The method according to any one of claims 1 to 5, wherein: The hydrophobic agent is selected from fatty acids with a carbon chain length of C8 or more; and the general formula is (RO) x R' 4-x Si alkoxysilane, wherein R is independently selected from C1-4 alkyl, R' is independently selected from C8-20 saturated or unsaturated, linear or branched alkyl, or 5-14 membered aromatic group, and x is selected from integers of 1-3; Preferably, the fatty acid with a carbon chain length of C8 or more is selected from C8-20 fatty acids, R is independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, and R' is independently selected from octadecyl, n-octyl, phenyl, benzyl, phenethyl; More preferably, the fatty acid with a carbon chain length of C8 or more is selected from caprylic acid, capric acid, stearic acid, and lauric acid; Most preferably, the hydrophobic agent is selected from stearic acid, dimethyldimethoxysilane, dimethoxydiphenylsilane, n-octyltriethoxysilane.
7. The method according to any one of claims 1 to 6, wherein: In step (3), the hydrophobic modification is performed using one or more of the following conditions: The organic solvent used to dissolve the hydrophobic agent is selected from one or more of methanol, ethanol, ethylene glycol, propanol, N,N-dimethylformamide (DMF), benzene, toluene, xylene, and cyclohexane, wherein preferably, the mass-to-volume ratio of the hydrophobic agent to the organic solvent is 1:100 to 1:30; The mass ratio of the hydrophobic agent to the catalyst is (0.05-0.5):1; The temperature of hydrophobic modification is 80℃-160℃, and the time is 1-12 hours; During the hydrophobic modification process, one or more of ultrasonic treatment, condensation reflux or stirring is simultaneously performed; The washing solvent is one or more of cyclohexane, toluene, xylene and ethanol.
8. The method according to any one of claims 1 to 7, wherein: In step (4), the drying conditions are 80-200° C., preferably 100-200° C., for 2-12 hours in air or nitrogen atmosphere.
9. A hydrophobic Fischer-Tropsch synthesis catalyst, wherein the hydrophobic Fischer-Tropsch synthesis catalyst is prepared by the method according to any one of claims 1 to 8.
10. A Fischer-Tropsch synthesis reaction method, comprising using a hydrophobic Fischer-Tropsch synthesis catalyst prepared by the method of any one of claims 1 to 8 to catalyze synthesis gas to carry out a Fischer-Tropsch synthesis reaction to prepare hydrocarbon compounds.
Citation Information
Patent Citations
Catalyst for inhibiting generation of C1 by-products in Fischer-Tropsch synthesis process and preparation method of catalyst
CN112007655A
Method for preparing oil product through synthesis gas hydrogenation
CN114768823A
Iron-based catalyst for Fischer-Tropsch synthesis as well as preparation method and application of iron-based catalyst
CN116116426A
High-stability Fischer-Tropsch synthesis iron-based catalyst and application thereof
CN116920892A
Hydrophobic organic modification of Co group Fischer-Tropsch synthesized catalyst, preparing and applications thereof
CN101224430A
Cited By
Method for preparing hydrophobic iron-based catalyst by using ball milling and ultrasonic chemical method and Fischer-Tropsch synthesis application of hydrophobic iron-based catalyst
CN119680543A
Efficient hydrophobic methanol catalyst and preparation method thereof
CN121623801A