Construction and application of photocatalytic system containing homogeneous promoter
By adding Ni ions and ligand to form a homogeneous nickel (II) complex cocatalyst, the problems of narrow absorption range and low catalytic activity of the titanium oxide photocatalyst are solved, and efficient photocatalytic activity and products are achieved Selective, suitable for dehalogenation coupling reaction.
Patent Information
- Application Number
- CN202310549153.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-16
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-05-16
AI Technical Summary
During the photocatalysis process, titanium oxide has a narrow light absorption range, weak light absorption capacity, and surface inhomogeneity and interphase diffusion resistance in the heterogeneous catalytic system, resulting in low catalytic activity and low selectivity of the target product.
By adding Ni ions and ligand to the reaction system to form a stable homogeneous nickel (II) complex cocatalyst, it acts as a support for TiO2 to prevent Ni from deposition on the surface of the titanium oxide catalyst, and constructs a homogeneous photocatalyst to improve the dispersion of the catalyst. and light absorption capacity.
It improves photocatalytic activity and target product selectivity, widens the spectral response range, and has excellent chemical stability, which is suitable for dehalogenation coupling reactions.
Smart Images

Figure SMS_1 
Figure HDA0004230707810000011 
Figure HDA0004230707810000012
Abstract
Description
Technical Field
[0001] The invention relates to the construction and application of a photocatalytic system containing a homogeneous promoter, and belongs to the technical field of photocatalytic materials and preparation thereof. Background Art
[0002] Using semiconductors as catalysts to convert solar energy into chemical energy is a process that is difficult to achieve with traditional thermal catalysis and has attracted great attention from researchers. However, there are also many problems in the semiconductor photocatalytic process, including low efficiency of photocatalytic conversion, easy recombination of carriers, low quantum yield, low stability of catalysts, etc., which greatly hinder the practical application of photocatalysis. At present, the introduction of co-catalysts on semiconductors can often improve the light absorption properties of semiconductors, regulate the energy band structure of catalysts, and inhibit the recombination of photogenerated electrons and holes. Therefore, by adding homogeneous co-catalysts, it is beneficial to improve the catalytic activity and improve the selectivity of target products.
[0003] Titanium oxide has a wide band gap, high energy and strong migration ability of photogenerated carriers, strong redox ability, and strong photocatalytic activity under ultraviolet light irradiation; however, its light absorption range is narrow and its light absorption ability is weak, which greatly reduces its practical value. In addition, in a heterogeneous catalytic system, there is a phase interface between titanium oxide and the reaction substrate, which is affected by surface heterogeneity and large interphase diffusion resistance. Therefore, adding a homogeneous co-catalyst to construct an oxidation / reduction active site is one of the effective ways to improve catalytic activity and selectivity of target products. The present invention constructs a homogeneous nickel (II) complex co-catalyst by adding a ligand to the reaction system, prevents the deposition of the co-catalyst Ni on the surface of the titanium oxide catalyst, overcomes the influence of surface heterogeneity and interphase diffusion of the heterogeneous catalytic system, ensures the dispersion and balance of the catalyst in the system, and improves the light absorption capacity. Its unique electronic energy band structure is suitable for dehalogenation coupling reactions, and it has excellent chemical stability. It is a new catalytic material worthy of development and promotion in the field of photocatalytic materials.
[0004] Although Ni / TiO 2 Composite photocatalysts, such as [Xiangze Du, Yong Peng, Josep Albero, Dan Li, Changwei Hu, Hermenegildo García. Synthetic. Fuels from Biomass: Photocatalytic Hydrodecarboxylation of Octanoic Acid by NiNanoparticles Deposited on TiO 2 .ChemSusChem, 2022, 15(2): 202102107.] etc.2 As the carrier, nickel salt is the Ni ion source, and by adding ligands, a homogeneous nickel (II) complex co-catalyst is formed. The application of this co-catalyst in dehalogenation coupling reaction has not been reported yet. Summary of the invention
[0005] The purpose of the present invention is to provide an innovative, simple and mild synthesis method, by adding Ni ions to form a stable complex with ligands to prevent Ni from being deposited in situ on TiO 2 Surface, synthesized homogeneous nickel (II) complex co-catalyst material for photocatalytic titanium oxidation.
[0006] The construction and application of a photocatalytic system containing a homogeneous promoter provided by the present invention include the following contents:
[0007] Using TiO 2 As a carrier, nickel salt is used as a Ni ion source, and a ligand is added to form a homogeneous nickel (II) complex catalyst. Methanol is used as a reducing agent, and an alkaline salt is added to neutralize hydrogen protons, which is applied to the dehalogenation coupling reaction. Its preparation includes the following steps:
[0008] (1) TiO 2 , nickel salts are added into the reaction tube. Nickel salts include nickel sulfate, nickel chloride, nickel nitrate, nickel bromide, nickel hydroxide, and nickel acetylacetonate. TiO 2 The molar ratio of the nickel salt is 0.333 to 200;
[0009] (2) Weighing an alkali additive and adding it to the reaction tube described in step (1). The alkali additive includes potassium carbonate, potassium bicarbonate, potassium bisulfate, sodium carbonate, sodium bicarbonate, sodium bisulfate, sodium formate, and sodium acetate. 2 The amount of substance ratio is 0.02 to 4;
[0010] (3) measuring methanol, and then adding it to acetonitrile to obtain a methanol-acetonitrile solution, wherein the volume ratio of acetonitrile to methanol is 0.667 to 30;
[0011] (4) adding the mixed solution of methanol and acetonitrile in step (3) into the reaction tube in step (2) with a volume of 1 mL;
[0012] (5) Measure the ligand and add it to the reaction tube of step (4). The ligand includes o-phenanthroline, biimidazole, bipyridine, terpyridine, 2,4,6-tripyridyl triazine, tetraphenylporphyrin and products of different substituents of the above substances. 2 The amount of substance ratio is 0.013 to 3;
[0013] (6) replacing the reaction tube obtained in step (5) with an inert gas of 0.05 to 3 MPa, including argon (Ar), nitrogen (N 2 );
[0014] (7) Using a xenon lamp or an LED lamp as a light source, irradiate the sample in the reaction tube of step (6) for 0.1 to 72 hours to obtain a TiO 2 Homogeneous photocatalyst.
[0015] In step (1), the nickel salt includes: nickel sulfate, nickel chloride, nickel nitrate, nickel bromide, nickelous hydroxide, nickel acetylacetonate. 2 The molar ratio of the amount of the nickel salt is preferably 5 to 20.
[0016] In step (2), the alkali additive includes potassium carbonate, potassium bicarbonate, potassium bisulfate, sodium carbonate, sodium bicarbonate, sodium bisulfate, sodium formate, and sodium acetate. The alkali additive is potassium carbonate, which reacts with TiO 2 The molar ratio of is preferably 0.4 to 1.
[0017] In step (3), the volume ratio of acetonitrile to methanol is preferably 1.5 to 19.
[0018] In step (4), when TiO 2 When the dosage is 8.0 mg, the volume of the mixed solution is preferably 1 to 1.5 mL.
[0019] In step (5), the ligand includes: o-phenanthroline, biimidazole, bipyridine, terpyridine, 2,4,6-tripyridyl triazine, tetraphenylporphyrin and products of different substituents of the above substances. The ligand is o-phenanthroline, and the ligand is in a state of being ... 2 The molar ratio of is preferably 0.05 to 0.2.
[0020] In step (6), the gas introduced into the reaction tube is preferably 0.1 to 1 MPa N 2 .
[0021] In step (7), a xenon lamp is used as a light source to irradiate the sample in the reaction tube of step (6) for a certain period of time to obtain a TiO 2 Homogeneous photocatalyst, wherein the illumination time is preferably 1 to 6 hours.
[0022] The nickel (II) complex prepared by the above preparation method is a homogeneous catalyst TiO 2 Photocatalyst systems.
[0023] Application of the above catalytic system in photocatalytic dehalogenation coupling reaction.
[0024] The present invention is the first to prepare TiO2 using nickel (II) complex as a co-catalyst. 2 The homogeneous photocatalyst constructs a homogeneous co-catalyst by adding a ligand to the reaction system, prevents the co-catalyst Ni from being deposited on the surface of the titanium oxide catalyst, overcomes the influence of the surface heterogeneity and interphase diffusion of the multiphase catalytic system, ensures the dispersion and balance of the catalyst in the system, and broadens the spectral response range. The light absorption capacity is improved. The preparation method of the present invention is simple, the reaction process is easy to control, the homogeneous photocatalytic titanium oxide co-catalyst composite photocatalyst has high catalytic activity, its unique electronic band structure is suitable for dehalogenation coupling reaction, and it has excellent chemical stability.
[0025] The homogeneous nickel (II) complex co-catalyst of the present invention has the characteristics of balanced stability and high catalytic activity. It is used for dehalogenation coupling reaction and can obtain dehalogenation coupling products with high selectivity. It also has simple preparation process and low manufacturing cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The XRD patterns of the catalysts before and after the reaction in Example 1 correspond to the TiO 2 Catalyst, TiO with nickel complex as co-catalyst after reaction 2 Homogeneous catalyst (with ligand) and Ni / TiO after reaction 2 Catalyst (without ligand).
[0027] Figure 2 HAADF-STEM and STEM-EDS images of the catalyst after the reaction in Example 1. Figure 2 a~b are TiO prepared in Example 1 with nickel complex as promoter 2 Homogeneous catalyst (with ligand) Figure 2 c~d are Ni / TiO prepared in Example 1 2 HAADF-STEM and STEM-EDS images of the catalyst (without ligand). DETAILED DESCRIPTION
[0028] Unless otherwise specified, the experimental methods used in the following embodiments of the present invention are conventional methods.
[0029] Unless otherwise specified, the materials, reagents, etc. used in the following examples of the present invention can be obtained from commercial sources.
[0030] The initial reactants used in the following examples of the present invention are commercially available analytically pure drugs.
[0031] In the following embodiments of the present invention, the crystal structure of the prepared material was tested by Malvern PANalytical Empirean X-ray diffractometer (XRD) (Cu Kα ray, voltage of 40 kV, current of 20 mA); the morphology and elemental composition of the prepared material were tested by a Talos F200X field emission transmission electron microscope (TEM) equipped with an energy dispersive spectrometer (EDS) (accelerating voltage of 200 kV) and an EDS spectrometer.
[0032] Embodiment 1:
[0033] TiO with o-phenanthroline-coordinated nickel(II) complex as co-catalyst 2 Preparation of homogeneous photocatalyst: weigh 8.0 mg TiO 2 , 39.4 mg nickel sulfate hexahydrate, and 34.6 mg potassium carbonate were added to a transparent quartz reaction tube; 0.1 mL methanol was measured and then added to 1 mL acetonitrile to obtain a methanol acetonitrile solution; 1 mL of the above methanol and acetonitrile mixed solution and 2.3 μL o-phenanthroline were measured and added to the above reaction tube; 0.3 Mpa N was introduced into the reaction tube. 2 Finally, a xenon lamp was used as the light source to irradiate the sample for 1 hour to obtain TiO 2 Homogeneous photocatalyst. The Ni(Ⅱ) complex and TiO 2 The molar ratio is 0.15:0.10.
[0034] The process and conditions are the same as in Example 1, except that no o-phenanthroline is added; when o-phenanthroline is not added, Ni is deposited on TiO 2 On the Ni / TiO 2 Heterogeneous photocatalysts.
[0035] Embodiment 2:
[0036] TiO with biimidazole-coordinated nickel(II) complex as cocatalyst 2 Preparation of homogeneous photocatalyst: weigh 8.0 mg TiO 2 , 39.4 mg nickel sulfate hexahydrate, and 34.6 mg potassium carbonate were added to a transparent quartz reaction tube; 0.1 mL methanol was measured and then added to 1 ml acetonitrile to obtain a methanol acetonitrile solution; 1 mL of the above methanol and acetonitrile mixed solution and 1.5 μL biimidazole were measured and added to the above reaction tube; 0.3 Mpa N was replaced in the reaction tube. 2 Finally, a xenon lamp was used as the light source to irradiate the sample for 1 hour to obtain TiO 2 Homogeneous photocatalyst. The Ni(Ⅱ) complex and TiO 2The molar ratio is 0.15:0.10.
[0037] The process and conditions are the same as in Example 2, except that no biimidazole is added. When no biimidazole is added, Ni is deposited on TiO 2 On the Ni / TiO 2 Heterogeneous photocatalysts.
[0038] Embodiment 3:
[0039] TiO with o-phenanthroline-coordinated nickel(II) complex as co-catalyst 2 Preparation of homogeneous photocatalyst: weigh 8.0 mg TiO 2 , 23.8.0 mg of nickel chloride hexahydrate, and 34.6 mg of potassium carbonate were added to a transparent quartz reaction tube; 0.1 mL of methanol was measured and then added to 1 mL of acetonitrile to obtain a methanol-acetonitrile solution; 1 mL of the above methanol-acetonitrile mixed solution and 2.3 μL of o-phenanthroline were measured and added to the above reaction tube; 0.3 Mpa of N was replaced in the reaction tube. 2 Finally, a xenon lamp was used as the light source to irradiate the sample for 1 hour to obtain TiO 2 Homogeneous photocatalyst. The Ni(Ⅱ) complex and TiO 2 The molar ratio is 0.15:0.10.
[0040] The process and conditions are the same as in Example 3, except that no o-phenanthroline is added. When o-phenanthroline is not added, Ni is deposited on TiO 2 On the Ni / TiO 2 Heterogeneous photocatalysts.
[0041] Embodiment 4:
[0042] TiO with o-phenanthroline-coordinated nickel(II) complex as co-catalyst 2 Preparation of homogeneous photocatalyst: weigh 8.0 mg TiO 2 , 39.4 mg nickel sulfate hexahydrate, and 20.5 mg sodium acetate were added to a transparent quartz reaction tube; 0.1 mL methanol was measured and then added to 1 mL acetonitrile to obtain a methanol acetonitrile solution; 1 mL of the above methanol and acetonitrile mixed solution and 2.3 μL o-phenanthroline were measured and added to the above reaction tube; 0.3 Mpa N was introduced into the reaction tube. 2 Finally, a xenon lamp was used as the light source to irradiate the sample for 1 hour to obtain TiO 2 Homogeneous photocatalyst. The Ni(Ⅱ) complex and TiO 2 The molar ratio is 0.15:0.10.
[0043] The process and conditions are the same as in Example 4, except that no o-phenanthroline is added; when o-phenanthroline is not added, Ni is deposited on TiO 2 On the Ni / TiO 2 Heterogeneous photocatalysts.
[0044] Embodiment 5:
[0045] TiO with o-phenanthroline-coordinated nickel(II) complex as co-catalyst 2 Preparation of homogeneous photocatalyst: weigh 8.0 mg TiO 2 , 39.4 mg nickel sulfate hexahydrate, and 34.6 mg potassium carbonate were added to a transparent quartz reaction tube; 0.1 mL methanol was measured and then added to 1 mL acetonitrile to obtain a methanol-acetonitrile solution; 1 mL of the above methanol-acetonitrile mixed solution and 3.45 μL o-phenanthroline were measured and added to the above reaction tube; 1.5 MPa of N was replaced in the reaction tube. 2 Finally, a xenon lamp was used as the light source to irradiate the sample for 1 hour to obtain TiO 2 Homogeneous photocatalyst. The Ni(Ⅱ) complex and TiO 2 The molar ratio is 0.15:0.10.
[0046] Embodiment 6:
[0047] TiO with biimidazole-coordinated nickel(II) complex as cocatalyst 2 Preparation of homogeneous photocatalyst: weigh 8.0 mg TiO 2 , 39.4 mg nickel sulfate hexahydrate, and 34.6 mg potassium carbonate were added to a transparent quartz reaction tube; 0.1 mL methanol was measured and then added to 1 mL acetonitrile to obtain a methanol-acetonitrile solution; 1 mL of the above methanol-acetonitrile mixed solution and 3 μL biimidazole were measured and added to the above reaction tube; 0.3 Mpa N was replaced in the reaction tube. 2 Finally, a xenon lamp was used as the light source to irradiate the sample for 1 hour to obtain TiO 2 Homogeneous photocatalyst. The Ni(Ⅱ) complex and TiO 2 The molar ratio is 0.15:0.10.
[0048] The process and conditions are the same as in Example 6, except that no biimidazole is added. When no biimidazole is added, Ni is deposited on TiO 2 On the Ni / TiO 2 Heterogeneous photocatalysts.
[0049] Embodiment 7:
[0050] TiO with o-phenanthroline-coordinated nickel(II) complex as co-catalyst 2 Preparation of homogeneous photocatalyst: weigh 8.0 mg TiO 2 , 35.7 mg nickel chloride hexahydrate, and 34.6 mg potassium carbonate were added to a transparent quartz reaction tube; 0.1 mL methanol was measured and then added to 1 mL acetonitrile to obtain a methanol acetonitrile solution; 1 mL of the above methanol and acetonitrile mixed solution and 2.3 μL o-phenanthroline were measured and added to the above reaction tube; 0.3 Mpa N was introduced into the reaction tube. 2 Finally, a xenon lamp was used as the light source to irradiate the sample for 1 hour to obtain TiO 2 Homogeneous photocatalyst. The Ni(Ⅱ) complex and TiO 2 The molar ratio is 0.15:0.10.
[0051] The process and conditions are the same as in Example 7, except that no o-phenanthroline is added; when o-phenanthroline is not added, Ni is deposited on TiO 2 On the Ni / TiO 2 Heterogeneous photocatalysts.
[0052] Embodiment 8:
[0053] TiO with o-phenanthroline-coordinated nickel(II) complex as co-catalyst 2 Preparation of homogeneous photocatalyst: weigh 8 mg TiO 2 , 39.4 mg nickel sulfate hexahydrate, and 30.8.0 mg sodium acetate were added to a transparent quartz reaction tube; 0.1 mL methanol was measured and then added to 1 mL acetonitrile to obtain a methanol acetonitrile solution; 1 mL of the above methanol and acetonitrile mixed solution and 2.3 μL o-phenanthroline were measured and added to the above reaction tube; 0.3 Mpa N was replaced in the reaction tube. 2 Finally, a xenon lamp was used as the light source to irradiate the sample for 1 hour to obtain TiO 2 Homogeneous photocatalyst. The Ni(Ⅱ) complex and TiO 2 The molar ratio is 0.15:0.10.
[0054] The process and conditions are the same as in Example 8, except that no o-phenanthroline is added; when o-phenanthroline is not added, Ni is deposited on TiO 2 On the Ni / TiO 2 Heterogeneous photocatalysts.
[0055] Embodiment 9:
[0056] Ligand-free Ni / TiO 2Preparation of heterogeneous photocatalyst: Weigh 8.0 mg TiO 2 , 39.4 mg nickel sulfate hexahydrate, and 34.6 mg potassium carbonate were added to a transparent quartz reaction tube; 0.1 mL methanol was measured and then added to 1 mL acetonitrile to obtain a methanol-acetonitrile solution; 1 ml of the above methanol-acetonitrile mixed solution was measured and added to the above reaction tube; 0.3 Mpa N was introduced into the reaction tube to replace 2 Finally, a xenon lamp was used as the light source to irradiate the sample for 1 hour, and Ni was deposited on the TiO 2 The ligand-free Ni / TiO 2 Heterogeneous photocatalyst. The Ni(Ⅱ) complex and TiO 2 The molar ratio is 0.15:0.10.
[0057] Embodiment 10:
[0058] Nickel-free TiO 2 Preparation of photocatalyst: weigh 8.0 mg TiO 2 , 34.6 mg potassium carbonate were added to a transparent quartz reaction tube; 0.1 mL methanol was measured and then added to 1 mL acetonitrile to obtain a methanol acetonitrile solution; 1 mL of the above methanol and acetonitrile mixed solution and 2.3 μL o-phenanthroline were measured and added to the above reaction tube; 0.3 Mpa N was replaced in the reaction tube. 2 Finally, a xenon lamp was used as the light source to irradiate the sample for 1 hour to obtain TiO 2 Photocatalyst.
[0059] Embodiment 11:
[0060] Nickel-free and ligand-free TiO 2 Preparation of photocatalyst: weigh 8.0 mg TiO 2 , 34.6 mg potassium carbonate were added to a transparent quartz reaction tube; 0.1 mL methanol was measured and then added to 1 mL acetonitrile to obtain a methanol-acetonitrile solution; 1 mL of the above methanol-acetonitrile mixed solution was measured and added to the above reaction tube; 0.3 Mpa N was introduced into the reaction tube to replace 2 Finally, a xenon lamp was used as the light source to irradiate the sample for 1 hour to obtain TiO 2 Photocatalyst.
[0061] Embodiment 12:
[0062] TiO with o-phenanthroline-coordinated nickel(II) complex as co-catalyst 2 Preparation of homogeneous photocatalyst: weigh 8.0 mg TiO 2and 39.4 mg of nickel sulfate hexahydrate were added to a transparent quartz reaction tube; 0.1 mL of methanol was measured and then added to 1 mL of acetonitrile to obtain a methanol-acetonitrile solution; 1 mL of the above methanol-acetonitrile mixed solution and 2.3 μL of o-phenanthroline were measured and added to the above reaction tube; 0.3 Mpa of N was replaced in the reaction tube. 2 Finally, a xenon lamp was used as the light source to irradiate the sample for 1 hour to obtain TiO 2 Homogeneous photocatalyst. The Ni(Ⅱ) complex and TiO 2 The molar ratio is 0.15:0.10.
[0063] The process and conditions are the same as in Example 12, except that o-phenanthroline is not added; when o-phenanthroline is not added, Ni is deposited on TiO 2 On the Ni / TiO 2 Heterogeneous photocatalysts.
[0064] Embodiment 13:
[0065] TiO with o-phenanthroline-coordinated nickel(II) complex as co-catalyst 2 Preparation of homogeneous photocatalyst: weigh 8.0 mg TiO 2 , 39.4 mg nickel sulfate hexahydrate, and 34.6 mg potassium carbonate were added to a transparent quartz reaction tube; 1 mL acetonitrile and 2.3 μL o-phenanthroline were added to the above reaction tube; 0.3 Mpa N was introduced into the reaction tube. 2 Finally, a xenon lamp was used as the light source to irradiate the sample for 1 hour to obtain TiO 2 Homogeneous photocatalyst. The Ni(Ⅱ) complex and TiO 2 The molar ratio is 0.15:0.10.
[0066] The process and conditions are the same as in Example 13, except that no o-phenanthroline is added. When o-phenanthroline is not added, Ni is deposited on TiO 2 On the Ni / TiO 2 Heterogeneous photocatalysts.
[0067] Embodiment 14:
[0068] TiO with o-phenanthroline-coordinated nickel(II) complex as co-catalyst 2 Preparation of homogeneous photocatalyst: weigh 8.0 mg TiO 2, 78.9 mg nickel sulfate hexahydrate, and 0.3 mg potassium carbonate were added to a transparent quartz reaction tube; 0.067 mL methanol was measured and then added to 1 mL acetonitrile to obtain a methanol acetonitrile solution; 1 mL of the above methanol and acetonitrile mixed solution and 0.1 μL o-phenanthroline were measured and added to the above reaction tube; 0.3 Mpa N was introduced into the reaction tube to replace 2 Finally, a xenon lamp was used as the light source to irradiate the sample for 1 hour to obtain TiO 2 Homogeneous photocatalyst. Nickel sulfate hexahydrate and TiO 2 The molar ratio of potassium carbonate to TiO is 0.30:0.10. 2 The molar ratio of acetonitrile and methanol is 0.002:0.10, the volume ratio of acetonitrile and methanol is 0.067:0.10, and the volume ratio of o-phenanthroline and TiO 2 The molar ratio is 0.013:0.10.
[0069] The process and conditions are the same as in Example 14, except that no o-phenanthroline is added. When o-phenanthroline is not added, Ni is deposited on TiO 2 On the Ni / TiO 2 Heterogeneous photocatalysts.
[0070] Embodiment 15:
[0071] TiO with o-phenanthroline-coordinated nickel(II) complex as co-catalyst 2 Preparation of homogeneous photocatalyst: weigh 8.0 mg TiO 2 , 0.1 mg nickel sulfate hexahydrate, and 55.3 mg potassium carbonate were added to a transparent quartz reaction tube; 0.1 mL methanol was measured and then added to 3 mL acetonitrile to obtain a methanol acetonitrile solution; 1 mL of the above methanol and acetonitrile mixed solution and 78 μL of o-phenanthroline were measured and added to the above reaction tube; 0.3 Mpa N was replaced in the reaction tube. 2 Finally, a xenon lamp was used as the light source to irradiate the sample for 1 hour to obtain TiO 2 Homogeneous photocatalyst. Nickel sulfate hexahydrate and TiO 2 The molar ratio of potassium carbonate and TiO 2 The molar ratio of acetonitrile and methanol is 0.40:0.10, the volume ratio of acetonitrile and methanol is 3:0.10, and the volume ratio of o-phenanthroline and TiO 2 The molar ratio is 0.3:0.10.
[0072] The process and conditions are the same as in Example 15, except that no o-phenanthroline is added; when o-phenanthroline is not added, Ni is deposited on TiO 2 On the Ni / TiO 2Heterogeneous photocatalysts.
[0073] The catalysts obtained in Examples 1 to 15 were respectively applied to the dechlorination coupling reaction of 2-chloroethanol. 1 mL of the nickel (II) complex prepared in Examples 1 to 13 as a co-catalyst was taken. 2 The homogeneous photocatalyst was placed in a transparent quartz reaction tube, and 0.2 mmol of halohydrin (2-chloroethanol) was added. The atmosphere in the reaction tube was replaced with N 2 Then 0.3Mpa N 2 ; The sample was irradiated with a xenon lamp at 25°C for 6 hours to obtain a dehalogenation coupling product (1,4-butanediol). The sample was filtered through a nylon filter (to remove solid matter in the system), the filtrate was collected, and the amount of the product generated per unit time was quantified by chromatography. The reaction results are shown in the following table.
[0074]
[0075] Embodiment 16:
[0076] TiO with o-phenanthroline-coordinated nickel(II) complex as co-catalyst 2 Preparation of homogeneous photocatalyst: weigh 8.0 mg TiO 2 , 39.4 mg nickel sulfate hexahydrate, and 34.6 mg potassium carbonate were added to a transparent quartz reaction tube; 0.1 mL methanol was measured and then added to 1 mL acetonitrile to obtain a methanol acetonitrile solution; 1 mL of the above methanol and acetonitrile mixed solution and 2.3 μL o-phenanthroline were measured and added to the above reaction tube; 0.3 Mpa N was introduced into the reaction tube. 2 Finally, a xenon lamp was used as the light source to irradiate the sample for 1 hour to obtain TiO 2 Homogeneous photocatalyst. The Ni(Ⅱ) complex and TiO 2 The molar ratio is 0.15:0.10.
[0077] The process and conditions are the same as those in Example 1, except that the catalyst is used for the dechlorination coupling reaction of 1-chloroethanol as the reaction raw material to obtain the target product 2,3-butanediol.
[0078] Embodiment 17:
[0079] TiO with o-phenanthroline-coordinated nickel(II) complex as co-catalyst 2 Preparation of homogeneous photocatalyst: weigh 8.0 mg TiO 2, 39.4 mg nickel sulfate hexahydrate, and 34.6 mg potassium carbonate were added to a transparent quartz reaction tube; 0.1 mL methanol was measured and then added to 1 mL acetonitrile to obtain a methanol acetonitrile solution; 1 mL of the above methanol and acetonitrile mixed solution and 2.3 μL o-phenanthroline were measured and added to the above reaction tube; 0.3 Mpa N was introduced into the reaction tube. 2 Finally, a xenon lamp was used as the light source to irradiate the sample for 1 hour to obtain TiO 2 Homogeneous photocatalyst. The Ni(Ⅱ) complex and TiO 2 The molar ratio is 0.15:0.10.
[0080] The process and conditions are the same as those in Example 1, except that the catalyst is used for the deiodination coupling reaction of 2-iodoethanol as the reaction raw material to obtain the target product 1,4-butanediol.
[0081] The catalyst obtained in Example 1 was applied to the dechlorination coupling of 1-chloroethanol and the deiodination coupling of 2-iodoethanol, corresponding to Example 16 and Example 17, respectively. 1 mL of the nickel (II) complex prepared in Examples 16-17 was taken as a co-catalyst of TiO 2 The homogeneous photocatalyst was placed in a transparent quartz reaction tube, and 0.2 mmol of the above halohydrin (1-chloroethanol or 2-iodoethanol) was added respectively. The atmosphere in the reaction tube was replaced with N 2 Then 0.3Mpa N 2 ; The sample was irradiated with a xenon lamp at 25°C for 6 hours to obtain a dehalogenation coupling product. The product was filtered through a nylon filter (to remove solid matter in the system), the filtrate was collected, and the amount of the product generated per unit time was quantified by chromatography. The reaction results are shown in the following table.
[0082] name Reaction substrate Coupling product Conversion rate (%) Selectivity (%) Example 1 2-Chloroethanol 1,4-Butanediol 74 72 Example 16 1-Chloroethanol 2,3-Butanediol 70 69 Embodiment 17 2-Iodoethanol 1,4-Butanediol 68 66
[0083] like Figure 1 As shown, the three lines correspond to the TiO 2 XRD pattern of homogeneous photocatalyst. 2θ values of 25.2°, 37.8°, 48.0° and 62.7° correspond to TiO 2 (101), (004), (200) and (204) crystal planes.
[0084] like Figure 2 The TiO2 prepared by the present invention with a nickel complex as a co-catalyst is shown. 2 Homogeneous catalysts and Ni / TiO 2 HAADF-STEM and STEM-EDS images of heterogeneous catalysts, by Figure 2Figures a and b show that a small amount of Ni nanoparticles are deposited on the TiO 2 The surface of the TiO2 is uniformly distributed. This indicates that Ni is stabilized in the liquid phase by the ligand and is not easy to deposit on the TiO2 2 Surface. In contrast Figure 2 Figures c and d show that a large number of Ni nanoparticles are deposited on the TiO 2 The surface of the TiO 2 surface.
[0085] It should also be noted that the above is a detailed introduction to the construction and application of a photocatalytic system containing a homogeneous co-catalyst provided by the present invention. Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. It should be pointed out that the present invention is not limited to the specific details of the above embodiments. Without departing from the principles of the present invention, it can also be combined in any suitable manner to make several improvements and modifications to the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The present invention will not further explain various possible combinations.
Claims
1. A method for constructing a photocatalytic system containing a homogeneous promoter, characterized in that: TiO2 is used as a carrier, nickel salt is used as a Ni ion source, a ligand is added to form a homogeneous nickel (II) complex catalyst, methanol is used as a reducing agent, and an alkaline salt is added to neutralize hydrogen protons. The preparation thereof includes the following steps: (1) Adding TiO2 and nickel salt into a photoreaction tube; The molar ratio of TiO2 to nickel salt is 0.333 to 200; (2) weighing an alkaline additive and adding it to the reaction tube described in step (1); the molar ratio of the alkaline additive to TiO2 is 0.02 to 4; (3) measuring methanol and acetonitrile and mixing them to obtain a mixed solution, wherein the volume ratio of acetonitrile to methanol is 0.667 to 150; (4) adding the mixed solution of methanol and acetonitrile in step (3) into the reaction tube in step (2), wherein the volume of the mixed solution is 0.5 to 2 mL when the amount of TiO2 is 8.0 mg; (5) measuring a ligand and then adding it to the reaction tube of step (4); the molar ratio of the ligand to TiO2 is 0.005 to 3; (6) replacing the reaction tube obtained in step (5) with an inert atmosphere gas of 0.05 to 3 MPa; (7) Using a xenon lamp and / or an LED lamp as a light source, irradiate the reaction material in the reaction tube of step (6) for 0.1 to 72 hours to obtain a TiO2 homogeneous photocatalyst with a nickel (II) complex as a co-catalyst.
2. The method according to claim 1, characterized in that: In step (1), the nickel salt includes: one or more of nickel sulfate, nickel chloride, nickel nitrate, nickel bromide, nickelous hydroxide, and nickel acetylacetonate; The molar ratio of TiO2 to nickel salt is preferably 5 to 20.
3. The method according to claim 1, characterized in that: In step (2), the alkaline additive includes: one or more of potassium carbonate, potassium bicarbonate, potassium bisulfate, sodium carbonate, sodium bicarbonate, sodium bisulfate, sodium formate, and sodium acetate; Preferably the base additive is potassium carbonate; The molar ratio of the alkali additive to TiO2 is preferably 0.4 to 1.
4. The method according to claim 1, characterized in that: In step (3), the volume ratio of acetonitrile to methanol is preferably 1.5 to 19.
5. The method according to claim 1, characterized in that: In step (5), the ligand includes: one or more of o-phenanthroline, biimidazole, bipyridine, terpyridine, 2,4,6-tripyridyltriazine, tetraphenylporphyrin and products of the above substances substituted with different substituents; The preferred ligand is o-phenanthroline; The molar ratio of the ligand to TiO2 is preferably 0.05 to 0.
2.
6. The method according to claim 1, characterized in that: In step (6), the inert atmosphere gas includes one or both of argon (Ar) and nitrogen (N2); The gas introduced into the reaction tube for replacement is preferably 0.1-1 MPa N2.
7. The method according to claim 1, characterized in that: In step (7), a xenon lamp is used as a light source to irradiate the sample in the reaction tube of step (6) for a certain period of time to obtain a TiO2 homogeneous photocatalyst with a nickel (II) complex as a co-catalyst, wherein the irradiation time is preferably 1 to 6 hours.
8. A TiO2 photocatalyst system in which the nickel (II) complex obtained by the construction method according to any one of claims 1 to 7 is a homogeneous co-catalyst.
9. Use of the catalyst system according to claim 8 in a photocatalytic dehalogenation coupling reaction.
10. The use according to claim 9, characterized in that: The reaction raw material is chloroethanol, and the reaction conditions are: nitrogen as an inert protective gas, acetonitrile as a solvent, and the reaction is carried out under a xenon lamp light source for 1 to 6 hours.
Citation Information
Patent Citations
Nickel complex / TiO2 composite material as well as preparation method and application thereof
CN114471735A
Heterogeneous photo-enzyme coupling catalyst as well as preparation method and application thereof
CN116083411A
Semiconductor photocatalyst for the photocatalytic reforming of biomass derivatives for hydrogen generation, and preparation and use thereof
US20130224105A1
Photoactive catalyst based on non-precious metals deposited on titanium dioxide
WO2016162801A1