Method for preparing polyaniline ternary heteropolyacid composite material

By using devices and turbulent heating technology in polyaniline ternary heteropolyacid composite materials, the problem of insufficient dispersion of polyaniline is solved, its conductivity is significantly improved, and performance needs in the fields of photoelectric catalysis and energy storage are met.

CN118991075APending Publication Date: 2024-11-22LIAONING INST OF SCI & TECH
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411302597.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Polyaniline is insufficient dispersibility in polyaniline ternary heteropolyacid composite materials, resulting in poor conductivity and difficulty in meeting the needs of photoelectric catalysis and energy storage.

Method used

Using a device and method, the heteropolyacid-doped polyaniline is effective in acrylate polymer by simultaneously injecting polyaniline and heteropolyacid-doped material into the inner cavity of the shell, and using turbulent states and heating conditions. Disperse to form a high conductivity polyaniline trimetallic heteropolyacid composite material.

Benefits of technology

The conductivity of polyaniline ternary heteropolyacid composites has been significantly improved, and its performance in the fields of photoelectric catalysis and energy storage is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118991075A_ABST
    Figure CN118991075A_ABST
Patent Text Reader

Abstract

The invention provides a method for manufacturing a polyaniline ternary heteropolyacid composite material, the method is executed by using a device for manufacturing the polyaniline ternary heteropolyacid composite material, and the method comprises the following steps: 1) filling an inner cavity of a shell with a first material; (2) supplying a first material through a first feeding pipe and supplying a second material at the temperature of 0-3 DEG C through a second feeding part at the same flow speed, and enabling a discharging pipe to be in an open state; (3) the first feeding pipe, the second feeding part and the discharging pipe are in a closed state, so that heteropolyacid-doped polyaniline is formed by the second material within first preset time, and an acrylate polymer is formed by the first material around the heteropolyacid-doped polyaniline; and (4) heating the shell for a second preset time at a preset temperature through the heating part, so that the rest part of the first material is polymerized to form the acrylate polymer. According to the device disclosed by the invention, the dispersity of polyaniline in the polyaniline ternary heteropolyacid composite material can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Aspects of embodiments of the present disclosure relate to a method for manufacturing a polyaniline ternary heteropolyacid composite material. Background Art

[0002] Polyaniline is an important conductive polymer with excellent chemical stability, high conductivity and unique proton doping mechanism. Its structure and physical and chemical properties strongly depend on the synthesis and doping methods. Different proton acid doping will have different effects on the microstructure and properties of PANI.

[0003] By combining polyaniline with heteropolyacids (such as metal oxides), the conductivity of polyaniline can be effectively improved, thereby showing better performance in the fields of photoelectrocatalysis and energy storage. Summary of the invention

[0004] The object of the present disclosure is to provide a device for manufacturing a polyaniline ternary heteropolyacid composite material, which can improve the dispersibility of polyaniline in the polyaniline ternary heteropolyacid composite material.

[0005] Another object of the present disclosure is to provide a method for preparing a polyaniline ternary heteropolyacid composite material having high electrical conductivity.

[0006] According to one aspect of the present disclosure, there is provided an apparatus for manufacturing a polyaniline ternary heteropolyacid composite material, the apparatus comprising: a shell having an inner cavity for accommodating a material of the polyaniline ternary heteropolyacid composite material and an opening partially opened in a first direction; a door rotatably mounted at the opening of the shell to place the shell in a closed or open state; a first feed pipe passing through a first side wall of the shell in a second direction perpendicular to the first direction and communicating with the inner cavity to supply a first material of the polyaniline ternary heteropolyacid composite material to the inner cavity; a discharge pipe passing through a second side wall of the shell opposite to the first side wall in a second direction opposite to the first feed pipe and communicating with the inner cavity; a second feed portion comprising a first sub-feed pipe passing through the shell in the first direction, a second sub-feed pipe extending from an end of the first sub-feed pipe located in the inner cavity of the shell toward the discharge pipe along a second direction, and a nozzle disposed on the second sub-feed pipe to spray the second material of the polyaniline ternary heteropolyacid composite material toward the discharge pipe; and a heating portion disposed outside the shell to heat the material of the polyaniline ternary heteropolyacid composite material in the inner cavity of the shell.

[0007] According to an embodiment of the present disclosure, the second feed portion may be disposed close to the first feed pipe, and the nozzle may be located on an extension line between the first feed pipe and the discharge pipe in the second direction.

[0008] According to an embodiment of the present disclosure, the nozzle may include: a main board having a through hole sleeved on the outer wall of a second sub-feed pipe; a sub-board arranged along the edge of the main board and extending from the edge of the main board toward the discharge pipe; and a nozzle arranged on the sub-board and having a plurality of holes.

[0009] According to an embodiment of the present disclosure, the plurality of holes may be arranged along a first direction and a third direction perpendicular to the first direction and the second direction.

[0010] According to an embodiment of the present disclosure, the shortest distance between adjacent holes among the plurality of holes may be between 1 mm and 2 mm.

[0011] According to an embodiment of the present disclosure, a hole diameter of each of the plurality of holes may be 0.5 mm to 1 mm.

[0012] According to an embodiment of the present disclosure, an inner diameter of the first feeding pipe and an inner diameter of the second sub-feeding pipe may be substantially equal.

[0013] According to an embodiment of the present disclosure, the second feeding part may further include a pump connected to the first sub-feeding pipe to supply the second material of the polyaniline ternary heteropolyacid composite material to the inner cavity.

[0014] According to an embodiment of the present disclosure, the device may further include a pump connected to the first feeding pipe to supply the first material of the polyaniline ternary heteropolyacid composite material to the inner cavity.

[0015] According to an embodiment of the present disclosure, the device may further include a valve disposed on the discharge pipe to place the discharge pipe in a closed or open state.

[0016] According to an embodiment of the present disclosure, the device may further include a flow meter disposed in the housing to monitor the flow rate of the first material in the housing in real time.

[0017] According to another aspect of the present disclosure, a method for manufacturing a polyaniline ternary heteropolyacid composite material is provided, the method being performed by using the above-mentioned device for manufacturing a polyaniline ternary heteropolyacid composite material, the method comprising the following steps: 1) filling the inner cavity of a shell with a first material, the first material comprising an acrylic monomer, an acrylic ester monomer, an ethylene glycol diacrylate crosslinking agent and a dibenzoyl peroxide initiator; 2) supplying the first material through a first feed pipe at the same flow rate while supplying a second material at a temperature of 0°C to 3°C through a second feed portion, and opening the discharge pipe, wherein the second material comprises aniline, a ternary heteropolyacid, ammonium persulfate and water; 3) closing the first feed pipe, the second feed portion and the discharge pipe so that the second material forms a heteropolyacid-doped polyaniline within a first predetermined time and the first material around the formed heteropolyacid-doped polyaniline forms an acrylic ester polymer; and 4) heating the shell at a predetermined temperature to a second predetermined time via a heating portion so that the remaining portion of the first material is polymerized to form an acrylic ester polymer, thereby forming the polyaniline ternary heteropolyacid composite material.

[0018] According to an embodiment of the present disclosure, the flow rate satisfies a Re value greater than 4000, wherein the Re value is expressed by the following formula:

[0019]

[0020] Wherein, Re is the Reynolds number; d is the diameter or equivalent diameter of the shell, in m; u is the flow rate of the first material, in m / s; ρ is the density of the acrylic monomer, in kg / m 3 ; μ is the viscosity of acrylic monomer, unit N·m -2 ·s.

[0021] According to an embodiment of the present disclosure, the first predetermined time may be 1.5 hours to 3 hours.

[0022] According to an embodiment of the present disclosure, the predetermined temperature may be 50° C. to 60° C., and the second predetermined time may be 14 hours to 16 hours.

[0023] According to an embodiment of the present disclosure, the molar ratio of acrylic monomer, acrylate monomer and ethylene glycol diacrylate crosslinker in the first material may be 10:2:0.5, and the added amount of dibenzoyl peroxide initiator may be 1 wt % of the total weight of the monomers.

[0024] According to an embodiment of the present disclosure, the molar ratio of aniline, tribasic heteropoly acid and ammonium persulfate in the second material may be 1:0.01-0.03:1.4, and the amount of water added may be 10 wt % of the total mass of aniline.

[0025] According to an embodiment of the present disclosure, step 2) may be performed for at least 1 minute or less than or equal to 2 minutes.

[0026] According to an embodiment of the present disclosure, the method further comprises: after polymerizing the first material, opening the door to take out the polyaniline ternary heteropoly acid composite material.

[0027] In the embodiment of the present disclosure, since the second material and the first material to form the heteropolyacid-doped polyaniline are injected simultaneously through the device of the present disclosure, and the first material is in a turbulent state, the second material is effectively dispersed by the first material in a turbulent state while forming the heteropolyacid-doped polyaniline, and the polymerization of the dispersed second material is in an exothermic state, causing the first material around it to undergo a polymerization reaction, thereby being able to fix the formed heteropolyacid-doped polyaniline without causing the heteropolyacid-doped polyaniline to aggregate, thereby improving the dispersibility of the heteropolyacid-doped polyaniline in the acrylic ester polymer. Therefore, the conductivity of the polyaniline ternary heteropolyacid composite material formed by the present disclosure is significantly increased. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The above and other aspects and features of the embodiments of the present disclosure will become more apparent through the following description in conjunction with the accompanying drawings, in which:

[0029] Figure 1 is a perspective view of an apparatus for manufacturing a polyaniline ternary heteropoly acid composite material according to an embodiment of the present disclosure;

[0030] Figure 2 is a schematic diagram of an apparatus for manufacturing a polyaniline ternary heteropoly acid composite material according to an embodiment of the present disclosure; and

[0031] Figure 3 4 is a schematic diagram of a second feeding part in a device for manufacturing a polyaniline ternary heteropolyacid composite material according to an embodiment of the present disclosure. DETAILED DESCRIPTION

[0032] Reference will now be made in detail to embodiments, examples of which are shown in the accompanying drawings. In this regard, the described embodiments may have different forms and should not be construed as being limited to the descriptions set forth herein. Therefore, the embodiments are described below only by reference to the accompanying drawings to explain aspects and features of the present description.

[0033] For ease of description, spatially relative terms such as "under", "below", "below", "above", "on", etc. may be used herein to describe the relationship of one element or feature to another element or features as shown in the figures. It will be understood that in addition to the orientation shown in the figures, the spatially relative terms are also intended to cover different orientations of the device in use or operation. For example, if the device in the figure is turned over, the elements described as "under" or "below" other elements or features will be oriented as "above" or "on" other elements or features. Therefore, the term "below" can cover both above and below orientations. The device can be oriented otherwise (rotated 90 degrees or in other orientations), and the spatially relative descriptors used herein should be interpreted accordingly.

[0034] Hereinafter, embodiments of the present disclosure will be described with reference to the accompanying drawings.

[0035] Figure 1 is a perspective view of an apparatus for manufacturing a polyaniline ternary heteropoly acid composite material according to an embodiment of the present disclosure; Figure 2 is a schematic diagram of an apparatus for manufacturing a polyaniline ternary heteropoly acid composite material according to an embodiment of the present disclosure; and Figure 3 4 is a schematic diagram of a second feeding part in a device for manufacturing a polyaniline ternary heteropolyacid composite material according to an embodiment of the present disclosure.

[0036] Reference Figure 1 , Figure 2 and Figure 3 The device for manufacturing a polyaniline ternary heteropoly acid composite material according to an embodiment of the present disclosure includes: a housing 100, a door 110, a second feed part 200, a first feed pipe 300, a discharge pipe 400 and a heating part.

[0037] The shell 100 can have a rectangular shape and have an inner cavity for accommodating a material of a polyaniline ternary heteropolyacid composite material, however, the embodiments of the present disclosure are not limited thereto, and the rectangular shape has two surfaces in a first direction Z, two other surfaces in a third direction Y perpendicular to the first direction Z, and two side walls in a second direction X perpendicular to the first direction Z and the third direction Y (for example, a first side wall and a second side wall opposite to each other).

[0038] In addition, in order to easily take out the formed polyaniline ternary heteropolyacid composite material from the housing 100 , an opening may be provided on the housing 100 . Specifically, the housing 100 may have a partially opened opening in the first direction Z.

[0039] Therefore, the case 100 may be formed of an insulating material (eg, glass, ceramic, etc.), however, the present disclosure is not limited thereto.

[0040] The door 110 may be rotatably mounted at the opening of the housing 100 to close or open the housing 100. Specifically, the door 110 may be connected to the opening of the housing 100 by a hinge so that the door 110 may be rotatably opened or closed relative to the housing 100.

[0041] In addition, the door 110 may be formed of the same insulating material as the housing 100 , however, the present disclosure is not limited thereto, and the door 110 may be formed of any suitable material as long as the door 110 is in an insulating state.

[0042] The first feed pipe 300 can pass through the first side wall of the housing 100 in the second direction X and communicate with the inner cavity to supply the first material of the polyaniline ternary heteropolyacid composite material to the inner cavity. In addition, in order to supply the first material, the first feed pipe 300 can be connected to a pump (eg, a peristaltic pump).

[0043] The discharge pipe 400 may pass through the second side wall of the housing opposite to the first side wall and communicate with the inner cavity in the second direction X. In addition, a valve may be provided on the discharge pipe 400 to close or open the discharge pipe.

[0044] The first feeding pipe 300 and the discharging pipe 400 may be formed of the same material.

[0045] Reference Figure 3 The second feed part 200 can supply the second material of the polyaniline ternary heteropoly acid composite material, and can include a first sub-feed pipe 210, a second sub-feed pipe 220 and a nozzle 230. In addition, in order to extend the contact time between the second material and the first material, preferably, the second feed part 230 can be arranged close to the first feed pipe 300.

[0046] The first sub-feed pipe 210 may pass through the housing 100 in the first direction Z to communicate with the inner cavity. Specifically, the first sub-feed pipe 210 may pass through a portion of the housing 100 in the first direction Z except for the opening.

[0047] The second sub-feed pipe 220 may extend from the end of the first sub-feed pipe 210 located in the inner cavity of the housing 100 along the second direction X toward the discharge pipe 400 .

[0048] In addition, the first and second feeding pipes 210 and 220 may be formed of the same material as the first feeding pipe 300 and the discharging pipe 400. Also, the first and second feeding pipes 210 and 220 may be integrally formed, however, the present disclosure is not limited thereto.

[0049] In addition, the diameter (eg, inner diameter) of the second sub-feed pipe 220 may be substantially the same as the diameter (eg, inner diameter) of the first feed pipe 300 , thereby facilitating control of the ratio between the first material and the second material.

[0050] The nozzle 230 may be disposed on the second sub-feed pipe 220 to spray the second material of the polyaniline ternary heteropoly acid composite material toward the discharge pipe 400. In addition, in order to improve the dispersibility of the second material in the first material, preferably, the nozzle 230 may be located on the extension line between the first feed pipe 300 and the discharge pipe 400 in the second direction X.

[0051] The nozzle 230 may include: a main board having a through hole sleeved on the outer wall of the second sub-feed pipe 220; a sub-board arranged along the edge of the main board and extending from the edge of the main board toward the discharge pipe 400; and a nozzle 240 arranged on the sub-board and having a plurality of holes.

[0052] The main board and the sub-board may be integrally formed, however, embodiments of the present disclosure are not limited thereto.

[0053] In addition, a plurality of holes may be arranged along the first direction Z and the third direction Y.

[0054] Furthermore, in order to improve the dispersibility of the second material in the first material, preferably, the shortest distance between adjacent holes among the plurality of holes may be between 1 mm and 2 mm, and the pore size of each of the plurality of holes may be between 0.5 mm and 1 mm.

[0055] In addition, the second feeding part 200 may further include a pump (eg, a peristaltic pump) connected to the first sub-feeding pipe 210 to supply the second material of the polyaniline ternary heteropoly acid composite material to the inner cavity.

[0056] According to an embodiment of the present disclosure, the apparatus may further include a flow meter (eg, a rectangular flow meter) disposed in the interior of the housing 100 to monitor the flow rate of the first material in the inner cavity.

[0057] The heating unit may be disposed outside the housing 100 to heat the material of the polyaniline ternary heteropoly acid composite material in the inner cavity of the housing 100 .

[0058] The device for manufacturing polyaniline ternary heteropolyacid composite material according to the embodiment of the present disclosure can improve the dispersibility of heteropolyacid-doped polyaniline formed by the second material in the acrylate polymer formed by the first material. Therefore, the conductivity of the polyaniline ternary heteropolyacid composite material formed by the present disclosure is significantly increased.

[0059] The process steps for producing the polyaniline ternary heteropolyacid composite material using the apparatus for producing the polyaniline ternary heteropolyacid composite material will be described below.

[0060] According to an embodiment of the present disclosure, a method for manufacturing a polyaniline ternary heteropolyacid composite material is performed by using the above-mentioned device for manufacturing a polyaniline ternary heteropolyacid composite material, and the method includes: step 1), filling the inner cavity of the shell with a first material; step 2), supplying the first material through a first feed pipe at the same flow rate and supplying a second material at a temperature of 0°C to 3°C through a second feed part, and opening the discharge pipe; step 3), closing the first feed pipe, the second feed part and the discharge pipe so that the second material forms heteropolyacid-doped polyaniline within a first predetermined time and the first material around the formed heteropolyacid-doped polyaniline forms an acrylate polymer; and step 4), heating the shell at a predetermined temperature to a second predetermined time via a heating part so that the remaining part of the first material is polymerized to form an acrylate polymer, thereby forming a polyaniline ternary heteropolyacid composite material.

[0061] In step 1), the inner cavity of the housing 100 is filled with the first material. Specifically, the inner cavity of the housing 100 can be filled with the first material through the first feeding pipe 300 by a peristaltic pump, or the door 110 can be opened to fill the inner cavity of the housing 100 with the first material through the opening of the housing 100. When the inner cavity of the housing 100 is filled with the first material through the first feeding pipe 300, the first material can be slowly injected to remove the gas in the inner cavity of the housing.

[0062] The first material can be used as a main component of the polyaniline ternary heteropoly acid composite material, and can include acrylic monomers, acrylic ester monomers, ethylene glycol diacrylate crosslinking agent, and dibenzoyl peroxide (BPO) initiator.

[0063] In an embodiment of the present disclosure, the acrylic monomer may include at least one of acrylic acid, methacrylic acid, ethylacrylic acid, propylacrylic acid, and isobutylacrylic acid. The acrylate monomer may include at least one of methyl methacrylate and ethyl methacrylate.

[0064] In an embodiment of the present disclosure, the ethylene glycol diacrylate cross-linking agent may include at least one of ethylene glycol diacrylate, ethylene glycol dimethacrylate, ethylene glycol diethyl acrylate, and ethylene glycol dipropyl acrylate.

[0065] In the embodiments of the present disclosure, dibenzoyl peroxide can initiate polymerization of the monomers of the first material without adversely affecting polymerization of the second material.

[0066] The acrylic monomer and the acrylate monomer may be polymerized at a predetermined temperature (eg, 55° C. to 60° C.) under the action of an initiator and a cross-linking agent to generate an acrylate polymer.

[0067] In an embodiment of the present disclosure, the molar ratio of acrylic monomer, acrylate monomer and ethylene glycol diacrylate crosslinker in the first material may be 10:2:0.5, and the added amount of dibenzoyl peroxide initiator may be 1 wt % of the total weight of the monomers.

[0068] After the inner cavity of the housing 100 is filled with the first material (step 1), the first material can be supplied at the same flow rate through the first feed pipe 300, and the second material at a temperature of 0° C. to 3° C. can be supplied through the second feed part 200, for example, by a peristaltic pump, that is, the first material and the second material are supplied together into the inner cavity of the housing 100. At the same time, the discharge pipe 400 is opened, so that the discharge pipe 400 is in an open state.

[0069] The second material can be used as a conductive agent for the polyaniline ternary heteropoly acid composite material, and can include aniline, ternary heteropoly acid, ammonium persulfate and water. In the embodiment of the present disclosure, the molar ratio of aniline, ternary heteropoly acid and ammonium persulfate in the second material can be 1:0.01 to 0.03:1.4, and the amount of water added can be 10wt% of the total mass of aniline.

[0070] In the embodiments of the present disclosure, the ternary heteropoly acid can be used as a dopant to dope the polymerized aniline, and can include H7SiW9V3O 40 In addition, ammonium persulfate is used as an initiator to polymerize aniline. Under the combined action of the ternary heteropoly acid and the initiator, heteropoly acid-doped polyaniline can be generated, thereby making the polyaniline conductive.

[0071] In addition, in the art, aniline, tribasic heteropoly acid and ammonium persulfate can usually initiate polymerization at a relatively low temperature. Therefore, in the present disclosure, in order to ensure that aniline, tribasic heteropoly acid and ammonium persulfate are polymerized in the shell or the first material in the shell, the second material can be placed at a temperature of 0°C to 3°C before the second material is supplied through the second feed part 200 to slow down the polymerization of aniline, tribasic heteropoly acid and ammonium persulfate in the second feed part to avoid clogging the nozzle 230. When the second material is supplied to the first material, the temperature is higher than 3°C, thereby increasing the polymerization reaction rate of the second material in the first material.

[0072] In the embodiment of the present disclosure, in order to make the second material have a better dispersion effect in the first material, the supply of the first material in the housing can be made turbulent. Specifically, the flow rate (m / s) of the first material can be controlled to satisfy the Re value greater than 4000, wherein the Re value is represented by the following formula:

[0073]

[0074] Wherein, Re is the Reynolds number; d is the diameter of the shell, in m; u is the flow rate of the first material, in m / s; ρ is the density of the acrylic monomer, in kg / m 3 ; μ is the viscosity of acrylic monomer, unit N·m -2 ·s.

[0075] In the present disclosure, since the first material is in a turbulent state, the second material supplied together with the first material is in a dispersed state driven by the first material, and the second material can undergo a polymerization reaction. The polymerization of the second material is an exothermic reaction, which can cause the first material around it to undergo a polymerization reaction as well, thereby fixing the heteropolyacid-doped polyaniline generated by the polymerization, and thereby better dispersing the heteropolyacid-doped polyaniline generated by the polymerization in the acrylic polymer formed by the polymerization of the first material.

[0076] In addition, in the embodiments of the present disclosure, if the flow rate of supplying the second material is lower than the flow rate of supplying the first material, the supply of the second material may be interrupted; if the flow rate of supplying the second material is higher than the flow rate of supplying the first material, a large amount of the second material may accumulate at the nozzle. Therefore, the first material and the second material need to be supplied at the same flow rate at the same time.

[0077] Furthermore, in order to improve the dispersibility of the second material in the first material, preferably, the shortest distance between adjacent holes among the plurality of holes is set between 1 mm and 2 mm, and the diameter of each hole is between 0.5 mm and 1 mm.

[0078] In addition, in order to achieve a balanced ratio between the first material and the second material in the housing 100, step 2) may be performed for at least 1 minute or less than or equal to 2 minutes.

[0079] In step 3), the first feed pipe, the second feed part and the discharge pipe are closed so that the second material completely forms the heteropolyacid-doped polyaniline within a first predetermined time (e.g., 1.5h to 3h). Since the temperature of the second material is higher than 3°C, the second material can start to accelerate polymerization, and the heat released by the polymerization of the second material can reach the polymerization reaction of the first material around it, so that the heteropolyacid-doped polyaniline can be fixed by the acrylic polymer generated around it. In addition, since the second material has been dispersed by the first material in a turbulent state, the heteropolyacid-doped polyaniline formed is also dispersed in the acrylic polymer formed by the first material.

[0080] In step 4), the shell may be heated by a heating unit at, for example, 50° C. to 60° C. for 14 to 16 hours, so that the remaining portion of the first material is completely polymerized, thereby forming a polyaniline ternary heteropoly acid composite material.

[0081] In addition, in the present disclosure, since different monomers require different curing times, after a period of curing, the polyaniline ternary heteropolyacid composite material is prepared in the shell. At this time, the door on the shell can be opened to take out the cured polyaniline ternary heteropolyacid composite material, thereby completing the preparation of the polyaniline ternary heteropolyacid composite material.

[0082] In the embodiments of the present disclosure, since the dispersibility of the polyaniline doped with heteropolyacid in the acrylic ester polymer is improved, the conductivity of the polyaniline ternary heteropolyacid composite material formed by the present disclosure is significantly increased, so that it can be used as a gel electrolyte. An example will be provided below for further explanation.

[0083] Example 1

[0084] First, the first material is pumped into the shell through a peristaltic pump. At the same time, the discharge port is closed to allow the first material to fill the internal space of the shell. The discharge port is opened, and the first material and the second material at a temperature of 3°C are injected into the shell at a constant flow rate of 4300mL / min. At the same time, a flow meter is used to measure the flow rate in the shell, and then the first material and the second material in the shell are balanced for 1 minute to reach a ratio. At this time, the second feed part, the discharge pipe, and the first feed pipe are closed. The second material in the shell begins to polymerize because it is higher than 3°C, and the acrylic monomers and acrylate monomers around it also begin to polymerize, so that the heteropolyacid-doped polyaniline formed by the second material is fixed by the acrylic polymer around it. After 2 hours, the polymerization of the second material is completed, and the temperature is heated to 60°C and maintained for 14 hours to polymerize the remaining first material, thereby completing the preparation of the polyaniline ternary heteropolyacid composite material. The results are shown in Table 1. The conductivity of the obtained polyaniline ternary heteropolyacid composite material is 3.0×10 - 4 S / cm.

[0085] The corresponding parameters of the device are as follows: the diameter of the shell is 2 cm, the shortest distance between adjacent holes among the holes is 1 mm, and the pore size of each hole is 0.5 mm, and the density and viscosity of acrylic acid are 1.051 g / cm 3 and 1.149 mPa·s. In addition, the ratio of the components used in the first material and the second material is shown in Table 1, wherein the amount of dibenzoyl peroxide initiator added is 1wt% of the total weight of the monomers, and the amount of water added is 10wt% of the total weight of aniline.

[0086] Example 2 and Example 3

[0087] Examples 2 and 3 were prepared in the same manner as in Example 1, except that the corresponding parameters of Table 1 were used.

[0088] Comparative Example 1

[0089] Comparative Example 1 was prepared in the same manner as in Example 1, except that the corresponding parameters of Table 1 were used.

[0090] Comparative Example 2

[0091] Aniline: ammonium persulfate: ternary heteropoly acid were mixed in water at a molar ratio of 1:1.4:0.01, stirred evenly by mechanical stirring, reacted at room temperature for 2 hours, and the ternary heteropoly acid doped polyaniline produced by the reaction was separated and added to a mixture of acrylic acid: methyl methacrylate: ethylene glycol diacrylate at a ratio of 10:2:0.5, and then 1wt% of the total weight of acrylic acid and acrylate monomers was added as dibenzoyl peroxide initiator, and the mixed solution was poured into a mold, left to stand for 2 hours, and then heated to 60°C for reaction for 12 hours. The results are shown in Table 1.

[0092] Table 1

[0093]

[0094] In Table 1, the ternary heteropoly acid is H7SiW9V3O 40 , where all ratios are molar ratios and the unit of conductivity is S / cm.

[0095] As can be seen from Table 1, when comparing Examples 1 to 3 with Comparative Example 1, it is found that the first material flow rate is too low to form a turbulent state well, causing the heteropoly acid-doped polyaniline to be unevenly dispersed in the acrylic polymer, so the conductivity of Comparative Example 1 is significantly lower than that of Examples 1 to 3. In addition, the conductivity of Examples 1 to 3 is significantly higher than that of Comparative Example 2, because the heteropoly acid-doped polyaniline with conductive properties is effectively dispersed in the polyaniline ternary heteropoly acid composite material, so that the conductivity can be significantly improved. However, the conductivity of Comparative Example 2 decreases due to the lack of dispersion arrangement during curing.

[0096] In summary, since the second material and the first material to be formed into the heteropolyacid-doped polyaniline are injected simultaneously through the device disclosed in the present invention, and the first material is in a turbulent state, the second material is effectively dispersed by the first material in a turbulent state while forming the heteropolyacid-doped polyaniline, and the polymerization of the dispersed second material is in an exothermic state, causing the first material around it to undergo a polymerization reaction, thereby being able to fix the formed heteropolyacid-doped polyaniline without causing the heteropolyacid-doped polyaniline to aggregate, thereby improving the dispersibility of the heteropolyacid-doped polyaniline in the acrylic ester polymer. Therefore, the conductivity of the polyaniline ternary heteropolyacid composite material formed by the present invention is significantly increased.

Claims

1. A method for preparing a polyaniline ternary heteropoly acid composite material, characterized in that: The method is performed by using an apparatus for manufacturing a polyaniline ternary heteropoly acid composite material. The device comprises: a shell having an inner cavity for accommodating a material of a polyaniline ternary heteropoly acid composite material and an opening partially opened in a first direction; a door rotatably mounted at the opening of the shell so that the shell is in a closed or open state; a first feed pipe passing through a first side wall of the shell in a second direction perpendicular to the first direction and communicating with the inner cavity to supply a first material of the polyaniline ternary heteropoly acid composite material to the inner cavity; a discharge pipe passing through a second side wall of the shell opposite to the first side wall in a second direction opposite to the first feed pipe and communicating with the inner cavity; a second feed portion comprising a first sub-feed pipe passing through the shell in the first direction, a second sub-feed pipe extending from an end of the first sub-feed pipe located in the inner cavity of the shell toward the discharge pipe along the second direction, and a nozzle arranged on the second sub-feed pipe to spray the second material of the polyaniline ternary heteropoly acid composite material toward the discharge pipe; and a heating portion arranged outside the shell to heat the material of the polyaniline ternary heteropoly acid composite material in the inner cavity of the shell, The method comprises the following steps: 1) filling the inner cavity of the shell with a first material, wherein the first material comprises an acrylic monomer, an acrylic ester monomer, an ethylene glycol diacrylate crosslinking agent and a dibenzoyl peroxide initiator; 2) supplying the first material through a first feed pipe at the same flow rate and supplying a second material at a temperature of 0°C to 3°C through a second feed portion, and opening the discharge pipe, wherein the second material comprises aniline, a ternary heteropoly acid, ammonium persulfate and water; 3) closing the first feed pipe, the second feed portion and the discharge pipe, so that the second material forms heteropoly acid-doped polyaniline within a first predetermined time and the first material around the formed heteropoly acid-doped polyaniline forms an acrylic ester polymer; and 4) heating the shell at a predetermined temperature to a second predetermined time via a heating portion, so that the remaining part of the first material is polymerized to form an acrylic ester polymer, thereby forming a polyaniline ternary heteropoly acid composite material.

2. The method according to claim 1, characterized in that The second feeding portion is arranged close to the first feeding pipe, and the nozzle is located on an extension line between the first feeding pipe and the discharging pipe in the second direction.

3. The method according to claim 1, characterized in that: The nozzle includes: a main board having a through hole sleeved on the outer wall of the second sub-feed pipe; a sub-board arranged along the edge of the main board and extending from the edge of the main board toward the discharge pipe; and a nozzle arranged on the sub-board and having a plurality of holes.

4. The method according to claim 3, characterized in that The plurality of holes are arranged along a first direction and a third direction perpendicular to the first direction and the second direction, The shortest distance between adjacent holes among the plurality of holes is between 1 mm and 2 mm, Each of the plurality of holes has a hole diameter of 0.5 mm to 1 mm.

5. The method according to claim 1, characterized in that The flow rate satisfies a Re value greater than 4000, wherein the Re value is expressed by the following formula: Wherein, Re is the Reynolds number; d is the diameter or equivalent diameter of the shell, in m; u is the flow rate of the first material, in m / s; ρ is the density of the acrylic monomer, in kg / m 3 ; μ is the viscosity of acrylic monomer, unit N·m -2 ·s.

6. The method according to claim 1, characterized in that The first predetermined time is 1.5 hours to 3 hours.

7. The method according to claim 1, characterized in that The predetermined temperature is 50° C. to 60° C., and the second predetermined time is 14 h to 16 h.

8. The method according to claim 1, characterized in that The molar ratio of acrylic acid monomer, acrylate monomer and ethylene glycol diacrylate crosslinking agent in the first material is 10:2:0.5, and the added amount of dibenzoyl peroxide initiator is 1wt% of the total weight of the monomers.

9. The method according to claim 1, characterized in that: The molar ratio of aniline, tribasic heteropoly acid and ammonium persulfate in the second material is 1:0.01-0.03:1.4, and the amount of water added is 10wt% of the total mass of aniline.

10. The method according to claim 1, characterized in that Perform step 2) for at least 1 minute or less than or equal to 2 minutes.

Citation Information

Cited By

  • Feed mixing mechanism and feed production line

    CN121103189A

  • Feed mixing mechanism and feed production line

    CN121103189B