Microporous low-thermal-conductivity composite silica brick and preparation method thereof

By combining the insulation layer of materials such as polylight pore silicon homogenizer in silicon bricks with traditional silicon brick working layer, the problems of high thermal conductivity and poor thermal insulation effect of silicon bricks are solved, and high strength and low thermal conductivity are achieved. Microporous low-thermal conductivity composite silicon bricks with good thermal insulation effect meet energy-saving needs in high temperature environments.

CN118993714AActive Publication Date: 2024-11-22湖北省中耐新材科技有限公司 +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411078661.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-22
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

The existing silicon bricks have high thermal conductivity and poor thermal insulation effect, making it difficult to effectively save energy and reduce consumption in high-temperature environments.

Method used

The thermal insulation layer consisting of polylight pore silicon homogenizer, quartz powder, silicon micropowder, sodium tripolyphosphate, sodium hexametaphosphate and binding agent is combined with the working layer of traditional silicon bricks, and the molding and firing process is optimized. , forming microporous and low thermal conductivity composite silicon bricks with high strength and low thermal conductivity.

Benefits of technology

It achieves high strength, low thermal conductivity and good thermal insulation effect, and synchronous molding and sintering can not only withstand high temperatures, but also save energy and reduce consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993714A_ABST
    Figure CN118993714A_ABST
Patent Text Reader

Abstract

The invention discloses a microporous low-thermal-conductivity composite silica brick and a preparation method thereof, and belongs to the technical field of composite silica bricks, a thermal insulation layer of the composite silica brick is prepared from the following components in percentage by mass: 65%-75% of a poly (light porous) siliceous homogenized material, 20%-25% of quartz powder, 2%-8% of silica powder, 0.1%-1% of sodium tripolyphosphate and the balance of water. The high-strength porous material formed by combining 0.05%-0.3% of sodium hexametaphosphate and 1%-2% of a binding agent II has the characteristics of high strength, low heat conductivity coefficient, good strength and heat preservation effect, energy conservation and consumption reduction; the working layer of the composite silica brick has the high strength of a traditional silica brick, is in direct contact with high-temperature materials, has the excellent performance of high-temperature wear resistance, high refractoriness under load, erosion resistance and thermal shock resistance, and achieves the use effect of stability and long service life. According to the invention, the high strength and thermal insulation effect of the composite silica brick are realized, and the energy-saving effects of synchronous molding, synchronous sintering, high temperature resistance and thermal insulation are realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite silica bricks, and in particular to a microporous low thermal conductivity composite silica brick and a preparation method thereof. Background Art

[0002] With the increasing shortage of energy, countries are paying more and more attention to the research, production and use of energy-saving materials for high-temperature industries. Silica bricks are a type of acidic refractory materials mainly composed of tridymite, cristobalite, and a small amount of residual quartz and glass phase. They have good resistance to acidic slag erosion, and the load softening temperature is as high as 1640-1670℃. The volume is relatively stable when used for a long time at high temperature. Silica bricks are mainly used for the partition walls of the carbonization chamber and combustion chamber of the coke oven, the regenerator and slag chamber of the steelmaking open hearth, the soaking furnace, the refractory materials of the glass melting furnace, and the vault and other load-bearing parts of the kiln such as the ceramic firing kiln. They are also used for the high-temperature load-bearing parts of the hot blast furnace and the top of the acid open hearth furnace.

[0003] Silica bricks are widely used and studied in refractory systems due to their high load softening temperature, good high temperature volume stability, and no shrinkage after long-term use. However, existing silica bricks have the problem of high thermal conductivity and poor thermal insulation effect. To this end, the present invention provides a microporous low thermal conductivity composite silica brick and a preparation method thereof. Summary of the invention

[0004] The present invention provides a microporous low thermal conductivity composite silica brick and a preparation method thereof, which effectively solves the technical problems of the existing silica bricks having high thermal conductivity and poor thermal insulation effect, and at the same time provides a microporous low thermal conductivity composite silica brick with high strength, low thermal conductivity, good thermal insulation effect, energy saving and consumption reduction.

[0005] The first object of the present invention is to provide a microporous low thermal conductivity composite silica brick, comprising a working layer and a thermal insulation layer, wherein the thermal insulation layer is wrapped outside the working layer; the thickness ratio of the working layer to the thermal insulation layer is 2-4:0.6-1.2;

[0006] The thermal insulation layer is composed of the following raw materials in percentage by mass: 65% to 75% of polyslightly porous siliceous homogenizing material, 20% to 25% of quartz powder, 2% to 8% of silicon powder, 0.1% to 1% of sodium tripolyphosphate, 0.05% to 0.3% of sodium hexametaphosphate, and 1% to 2% of binder II, totaling 100%.

[0007] As a preferred implementation, the thickness ratio of the working layer to the insulation layer is 2 to 4:1.

[0008] As a preferred embodiment, the binder II is phosphoric acid or a phosphate binder.

[0009] As a preferred embodiment, the working layer is composed of the following raw materials in the following mass percentages: 50% to 70% silica sand, 15% to 35% silicon powder, 1% to 2.5% binder I, 2% to 5% fluorite powder, 5% to 10% silicon micropowder, 0% to 1.5% iron scale powder, and 0% to 3% calcium oxide, totaling 100%.

[0010] As a preferred embodiment, the binder I is one or more of lignin, cellulose, dextrin, and phosphate.

[0011] The second object of the present invention is to provide a method for preparing a microporous low thermal conductivity composite silica brick, comprising the following steps:

[0012] Weigh the raw materials of the working layer and the insulation layer respectively;

[0013] Mix 50% to 70% by mass of silica sand, 15% to 35% of silica powder, 1% to 2.5% of binder I, 2% to 5% of fluorite powder, 5% to 10% of silicon micropowder, 0% to 1.5% of iron scale powder, and 0% to 3% of calcium oxide to obtain a working layer premix;

[0014] Mix 65% to 75% by mass of slightly porous siliceous homogenized material, 20% to 25% of quartz powder, 2% to 8% of silicon powder, 0.1% to 1% of sodium tripolyphosphate, 0.05% to 0.3% of sodium hexametaphosphate, and 1% to 2% of binder II to obtain a premix for the thermal insulation layer;

[0015] The working layer premix and the insulation layer premix are respectively loaded into the mold, separated by a template in the middle, and after filling, the template is removed, and then pressed into shape, dried to obtain a brick, and the brick is heated to 1300-1450°C, kept warm, and cooled.

[0016] As a preferred embodiment, during pressing, the pressure is 100-150 MPa and the time is 3-10 min.

[0017] As a preferred implementation, the insulation time is 5 to 15 hours.

[0018] As a preferred embodiment, it is characterized in that the temperature rising procedure is: heating to 200-600°C at 20°C / h, heating to 600-1100°C at 25°C / h, heating to 1100-1350°C at 7°C / h, and heating to 1300-1450°C at 1-3°C / h.

[0019] As a preferred implementation manner, the drying is specifically as follows: The drying is specifically as follows: placing the bricks in a drying kiln at 100-200°C to dry until the moisture content is less than 2%, and then loading the kiln for firing.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The present invention provides a microporous low thermal conductivity composite silica brick and a preparation method thereof. The thermal insulation layer used in the present invention is formed by combining 65% to 75% by mass of microporous siliceous homogenized material, 20% to 25% of quartz powder, 2% to 8% of silicon powder, 0.1% to 1% of sodium tripolyphosphate, 0.05% to 0.3% of sodium hexametaphosphate and 1% to 2% of binder II. The working layer has the high strength of traditional silica bricks, directly contacts high-temperature materials, has high-temperature wear resistance, high load softening temperature, corrosion resistance, and thermal shock resistance, achieving a stable and long-life use effect; the thermal insulation layer uses a special high-strength porous material, which has the characteristics of high strength, low thermal conductivity, good strength and thermal insulation effect, and energy saving and consumption reduction, thereby achieving the high strength and thermal insulation effect of the composite silica brick. The present invention realizes synchronous molding and synchronous firing, and has the energy-saving effect of both high temperature resistance and thermal insulation. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a physical picture of the microporous low thermal conductivity composite silicon brick prepared by the present invention. DETAILED DESCRIPTION

[0023] In order to enable those skilled in the art to better understand the technical solution of the present invention and implement it, the present invention is further described below in conjunction with specific embodiments and drawings, but the embodiments are not intended to limit the present invention. The following test methods and detection methods, unless otherwise specified, are conventional methods; the reagents and raw materials, unless otherwise specified, are commercially available.

[0024] The present invention mentioned in the background technology: Silica bricks are widely used and studied in refractory systems due to their high load softening temperature point, good high temperature volume stability, and no shrinkage after long-term use. However, the existing silica bricks have the problem of high thermal conductivity and poor thermal insulation effect. Based on the above technical problems, the present invention provides a microporous low thermal conductivity composite silica brick and a preparation method thereof. The thermal insulation layer used in the present invention is composed of 65% to 75% by mass of polyslightly porous siliceous homogenized material, 20% to 25% quartz powder, 2% to 8% silicon powder, 0.1% to 1% sodium tripolyphosphate, 0.05% to 0.3% sodium hexametaphosphate and 1% to 2% binder II. The working layer has the high strength, high temperature wear resistance, high load softening temperature, corrosion resistance, and thermal shock resistance of traditional silica bricks. The thermal insulation layer has the characteristics of high strength, low thermal conductivity, good strength and thermal insulation effect, energy saving and consumption reduction, and realizes synchronous molding and synchronous firing, which is both high temperature resistant and heat-insulating. Energy-saving effect.

[0025] The technical solution of the present invention is analyzed and explained in detail below.

[0026] The present invention first provides a microporous low thermal conductivity composite silica brick, comprising a working layer and a thermal insulation layer, wherein the thermal insulation layer is wrapped outside the working layer; the thickness ratio of the working layer to the thermal insulation layer is 2-4:0.6-1.2;

[0027] The thermal insulation layer is composed of the following raw materials in percentage by mass: 65% to 75% of polyslightly porous siliceous homogenizing material, 20% to 25% of quartz powder, 2% to 8% of silicon micropowder, 0.1% to 1% of sodium tripolyphosphate, 0.05% to 0.3% of sodium hexametaphosphate, and 1% to 2% of binder II, which totals 100%; wherein the polyslightly porous siliceous homogenizing material mainly has a heat-insulating effect, the fine powder and micropowder have a filling effect, the sodium tripolyphosphate and sodium hexametaphosphate are used as dispersants, and the binder provides the material with initial demolding strength.

[0028] The working layer is composed of the following raw materials in mass percentage: 50% to 70% silica sand, 15% to 35% silica powder, 1% to 2.5% binder I, 2% to 5% fluorite powder, 5% to 10% silicon micropowder, 0% to 1.5% iron scale powder, and 0% to 3% calcium oxide, totaling 100%. Among them, silica sand is the main component of the material and plays a role in the skeleton structure, fine powder and micropowder play a filling role, iron scale powder and calcium oxide are commonly used mineralizers to improve the microstructure of the material and enhance the material performance, and the binder provides the initial handling strength for the blank.

[0029] In order to further achieve the high strength and thermal insulation effect of the composite silica brick of the present invention, the thickness ratio of the working layer to the thermal insulation layer is 2 to 4:1.

[0030] In order to further achieve a good bonding effect between the components in the thermal insulation layer of the present invention, the binder II is phosphoric acid or a phosphate binder.

[0031] In order to further achieve a good bonding effect between the components in the working layer of the present invention, the binder I is one or more of lignin, cellulose, dextrin, and phosphate.

[0032] The present invention also provides a method for preparing a microporous low thermal conductivity composite silica brick, comprising the following steps:

[0033] Weigh the raw materials of the working layer and the insulation layer respectively;

[0034] Mix 50% to 70% by mass of silica sand, 15% to 35% of silica powder, 1% to 2.5% of binder I, 2% to 5% of fluorite powder, 5% to 10% of silicon micropowder, 0% to 1.5% of iron scale powder, and 0% to 3% of calcium oxide to obtain a working layer premix;

[0035] Mix 65% to 75% by mass of slightly porous siliceous homogenized material, 20% to 25% of quartz powder, 2% to 8% of silicon powder, 0.1% to 1% of sodium tripolyphosphate, 0.05% to 0.3% of sodium hexametaphosphate, and 1% to 2% of binder II to obtain a premix for the thermal insulation layer;

[0036] The working layer premix and the insulation layer premix are respectively loaded into the mold, separated by a template in the middle, and after filling, the template is removed, and then pressed into shape, dried to obtain a brick, and the brick is heated to 1300-1450°C, kept warm, and cooled.

[0037] In order to ensure a good bonding effect between the insulation layer and the working layer, the pressing pressure is 100-150MPa and the time is 3-10min.

[0038] In order to remove most of the moisture in the bricks before firing, so as to avoid the rapid evaporation of moisture in the subsequent heating process to affect the brick structure, and then destroy the mechanical strength and thermal insulation performance of the composite silicon bricks, the drying is specifically as follows: the bricks are placed in a drying kiln at 100-200°C and dried until the moisture is less than 2%, and then loaded into the kiln for firing.

[0039] In order to reduce the temperature difference caused by instantaneous heating and the crystal transformation of silicon oxide during the brick firing process, which may lead to cracks in the brick insulation layer and the working layer, the heating procedure is: heating to 200-600°C at 20°C / h, heating to 600-1100°C at 25°C / h, heating to 1100-1350°C at 7°C / h, and heating to 1300-1450°C at 1-3°C / h; the gradient heating method can maximize the reduction of cracks in the brick.

[0040] In order to improve the mechanical strength of the bricks during the firing process, the insulation time is 5 to 15 hours.

[0041] The effects are described below through specific embodiments and comparative examples.

[0042] Example 1

[0043] A microporous low thermal conductivity composite silica brick, the thermal insulation layer is composed of the following raw materials in percentage by mass: 65% (less than 8mm) of polyslightly porous siliceous homogenized material, 25% (less than 100μm) of quartz powder, 8% (less than 10μm) of silicon powder, 0.1% of sodium tripolyphosphate, 0.3% of sodium hexametaphosphate, 1.6% of binder II (phosphoric acid), a total of 100%;

[0044] The working layer is composed of the following raw materials in percentage by mass: 50% silica sand (1.5-3.0 mm), 35% silica powder (less than 100 μm), 1% binder I (lignin), 5% fluorite powder (less than 100 μm), 6% silicon micropowder (less than 10 μm), 1.0% iron scale powder (less than 100 μm), and 2% calcium oxide, totaling 100%.

[0045] The method for preparing the above-mentioned microporous low thermal conductivity composite silica brick comprises the following steps:

[0046] Weigh the raw materials of the working layer and the thermal insulation layer, premix the raw materials of the working layer and the thermal insulation layer respectively to obtain a working layer premix and a thermal insulation layer premix, respectively load the working layer premix and the thermal insulation layer premix into a mold, separate them with a template in the middle, remove the template after filling, and then press at 100MPa for 3min, and then place in a 100℃ drying kiln to dry until the moisture is less than 2% to obtain a brick, the thickness ratio of the working layer and the thermal insulation layer is 2:0.6, heat the brick to 1300℃, keep warm for 5h, and cool with the furnace to obtain;

[0047] The heating procedure is: heating to 200°C at 20°C / h, heating to 600°C at 25°C / h, heating to 1100°C at 7°C / h, and heating to 1300°C at 1-3°C / h.

[0048] Example 2

[0049] A microporous low thermal conductivity composite silica brick, the thermal insulation layer is composed of the following raw materials in percentage by mass: 75% (less than 8 mm) of polymicroporous siliceous homogenized material, 20% (less than 100 μm) of quartz powder, 2% (less than 10 μm) of silicon powder, 1% of sodium tripolyphosphate, 0.05% of sodium hexametaphosphate, 1.95% of binder II (aluminum dihydrogen phosphate), a total of 100%;

[0050] The working layer is composed of the following raw materials in percentage by mass: 70% silica sand (1.5-3.0 mm), 15% silica powder (less than 100 μm), 2.5% binder I (cellulose), 3% fluorite powder (less than 100 μm), 5% silicon micropowder (less than 10 μm), 1.5% iron scale powder (less than 100 μm), and 3% calcium oxide, totaling 100%.

[0051] The method for preparing the above-mentioned microporous low thermal conductivity composite silica brick comprises the following steps:

[0052] Weigh the raw materials of the working layer and the thermal insulation layer, premix the raw materials of the working layer and the thermal insulation layer respectively to obtain a working layer premix and a thermal insulation layer premix, respectively load the working layer premix and the thermal insulation layer premix into a mold, separate them with a template in the middle, remove the template after filling, and then press at 150MPa for 10min, and then place in a 200℃ drying kiln to dry until the moisture is less than 2% to obtain a brick, the thickness ratio of the working layer and the thermal insulation layer is 4:1.2, heat the brick to 1450℃, keep warm for 15h, and cool with the furnace to obtain;

[0053] The heating procedure is: heating to 600°C at 20°C / h, heating to 1100°C at 25°C / h, heating to 1350°C at 7°C / h, and heating to 1450°C at 1-3°C / h.

[0054] Example 3

[0055] A microporous low thermal conductivity composite silica brick, the thermal insulation layer is composed of the following raw materials in percentage by mass: 70% (less than 8mm) of polyslightly porous siliceous homogenized material, 22% (less than 100μm) of quartz powder, 6% (less than 10μm) of silicon powder, 0.5% of sodium tripolyphosphate, 0.3% of sodium hexametaphosphate, 1.2% of binder II (aluminum dihydrogen phosphate), a total of 100%;

[0056] The working layer is composed of the following raw materials in percentage by mass: 60% silica sand (1.5-3.0 mm), 25% silica powder (less than 100 μm), 2.0% binder I (dextrin), 4% fluorite powder (less than 100 μm), 5.5% silicon micropowder (less than 10 μm), 0.5% iron scale powder (less than 100 μm), and 3% calcium oxide, totaling 100%.

[0057] The method for preparing the above-mentioned microporous low thermal conductivity composite silica brick comprises the following steps:

[0058] Weigh the raw materials of the working layer and the thermal insulation layer, premix the raw materials of the working layer and the thermal insulation layer respectively to obtain a working layer premix and a thermal insulation layer premix, respectively load the working layer premix and the thermal insulation layer premix into molds, separate them with templates, remove the templates after filling, press at 120MPa for 7min, and then place in a 150°C drying kiln to dry until the moisture is less than 2% to obtain a brick, the thickness ratio of the working layer and the thermal insulation layer is 2:1, heat the brick to 1350°C, keep warm for 10h, and cool with the furnace to obtain;

[0059] The heating procedure is: heating to 400°C at 20°C / h, heating to 800°C at 25°C / h, heating to 1200°C at 7°C / h, and heating to 1350°C at 1-3°C / h.

[0060] Example 4

[0061] A microporous low thermal conductivity composite silica brick, the thermal insulation layer is composed of the following raw materials in percentage by mass: 68% (less than 8 mm) of polyslightly porous siliceous homogenized material, 24% (less than 100 μm) of quartz powder, 5% (less than 10 μm) of silicon powder, 0.8% of sodium tripolyphosphate, 0.2% of sodium hexametaphosphate, 2% of binder II (aluminum dihydrogen phosphate), a total of 100%;

[0062] The working layer is composed of the following raw materials in percentage by mass: 65% silica sand (1.5-3.0 mm), 20% silica powder (less than 100 μm), 1.5% binder I (phosphate), 5% fluorite powder (less than 100 μm), 5% silicon micropowder (less than 10 μm), 1.0% iron scale powder (less than 100 μm), and 2.5% calcium oxide, totaling 100%.

[0063] The method for preparing the above-mentioned microporous low thermal conductivity composite silica brick comprises the following steps:

[0064] Weigh the raw materials of the working layer and the thermal insulation layer, premix the raw materials of the working layer and the thermal insulation layer respectively to obtain a working layer premix and a thermal insulation layer premix, respectively load the working layer premix and the thermal insulation layer premix into molds, separate them with templates in the middle, remove the templates after filling, and then press at 140MPa for 5min, and then place in a 120°C drying kiln to dry until the moisture content is less than 2% to obtain a brick, the thickness ratio of the working layer and the thermal insulation layer is 4:1, heat the brick to 1400°C, keep warm for 12h, and cool with the furnace to obtain;

[0065] The heating procedure is: heating to 300°C at 20°C / h, heating to 700°C at 25°C / h, heating to 1300°C at 7°C / h, and heating to 1400°C at 1-3°C / h.

[0066] Example 5

[0067] A microporous low thermal conductivity composite silica brick, the thermal insulation layer is composed of the following raw materials in percentage by mass: 72% (less than 8 mm) of polymicroporous siliceous homogenized material, 20% (less than 100 μm) of quartz powder, 6% (less than 10 μm) of silicon powder, 0.2% of sodium tripolyphosphate, 0.3% of sodium hexametaphosphate, 1.5% of binder II (aluminum dihydrogen phosphate), a total of 100%;

[0068] The working layer is composed of the following raw materials in percentage by mass: 55% silica sand (1.5-3.0 mm), 30% silica powder (less than 100 μm), 2.5% binder I (lignin and cellulose in a mass ratio of 1:1), 4% fluorite powder (less than 100 μm), 6% silicon micropowder (less than 10 μm), 0.5% iron scale powder (less than 100 μm), and 2% calcium oxide, totaling 100%.

[0069] The method for preparing the above-mentioned microporous low thermal conductivity composite silica brick comprises the following steps:

[0070] Weigh the raw materials of the working layer and the thermal insulation layer, premix the raw materials of the working layer and the thermal insulation layer respectively to obtain a working layer premix and a thermal insulation layer premix, respectively load the working layer premix and the thermal insulation layer premix into molds, separate them with templates, remove the templates after filling, press at 110MPa for 4min, and then place in a 180°C drying kiln to dry until the moisture is less than 2% to obtain a brick, the thickness ratio of the working layer and the thermal insulation layer is 3:1, heat the brick to 1450°C, keep warm for 8h, and cool with the furnace to obtain;

[0071] The heating procedure is: heating to 500°C at 20°C / h, heating to 1000°C at 25°C / h, heating to 1150°C at 7°C / h, and heating to 1300°C at 1-3°C / h.

[0072] Example 6

[0073] A microporous low thermal conductivity composite silica brick, the thermal insulation layer is composed of the following raw materials in percentage by mass: 66% (less than 8mm) of polyslightly porous siliceous homogenized material, 25% (less than 100μm) of quartz powder, 7% (less than 10μm) of silicon powder, 0.9% of sodium tripolyphosphate, 0.1% of sodium hexametaphosphate, 1% of binder II (aluminum dihydrogen phosphate), a total of 100%;

[0074] The working layer is composed of the following raw materials in percentage by mass: 58% silica sand (1.5-3.0 mm), 28% silica powder (less than 100 μm), 2.0% binder I (cellulose, dextrin and phosphate in a mass ratio of 1:1:1), 3% fluorite powder (less than 100 μm), 6% silicon micropowder (less than 10 μm), 0.5% iron scale powder (less than 100 μm), and 2.5% calcium oxide, totaling 100%.

[0075] The method for preparing the above-mentioned microporous low thermal conductivity composite silica brick comprises the following steps:

[0076] Weigh the raw materials of the working layer and the thermal insulation layer, premix the raw materials of the working layer and the thermal insulation layer respectively to obtain a working layer premix and a thermal insulation layer premix, respectively load the working layer premix and the thermal insulation layer premix into a mold, separate them with a template in the middle, remove the template after filling, and then press at 100MPa for 10min, and then place in a 200℃ drying kiln to dry until the moisture is less than 2% to obtain a brick, the thickness ratio of the working layer and the thermal insulation layer is 2:1.2, heat the brick to 1400℃, keep warm for 6h, and cool with the furnace to obtain;

[0077] The heating procedure is: heating to 350°C at 20°C / h, heating to 900°C at 25°C / h, heating to 1250°C at 7°C / h, and heating to 1350°C at 1-3°C / h.

[0078] Example 7

[0079] A microporous low thermal conductivity composite silica brick, the thermal insulation layer is composed of the following raw materials in percentage by mass: 74% (less than 8mm) of polyslightly porous siliceous homogenized material, 21% (less than 100μm) of quartz powder, 2% (less than 10μm) of silicon powder, 0.7% of sodium tripolyphosphate, 0.3% of sodium hexametaphosphate, 2% of binder II (aluminum dihydrogen phosphate), a total of 100%;

[0080] The working layer is composed of the following raw materials in percentage by mass: 62% silica sand (1.5-3.0 mm), 30% silica powder (less than 100 μm), 1% binder I (cellulose and phosphate in a mass ratio of 1:1), 2% fluorite powder (less than 100 μm), 5% silicon micropowder (less than 10 μm), 0% iron scale powder (less than 100 μm), and 0% calcium oxide, totaling 100%.

[0081] The method for preparing the above-mentioned microporous low thermal conductivity composite silica brick comprises the following steps:

[0082] Weigh the raw materials of the working layer and the thermal insulation layer, premix the raw materials of the working layer and the thermal insulation layer respectively to obtain a working layer premix and a thermal insulation layer premix, respectively load the working layer premix and the thermal insulation layer premix into molds, separate them with templates, remove the templates after filling, press at 150MPa for 3min, and then place in a 100°C drying kiln to dry until the moisture is less than 2% to obtain a brick, the thickness ratio of the working layer and the thermal insulation layer is 4:0.6, heat the brick to 1300°C, keep warm for 14h, and cool with the furnace to obtain;

[0083] The heating procedure is: heating to 550°C at 20°C / h, heating to 850°C at 25°C / h, heating to 1200°C at 7°C / h, and heating to 1450°C at 1-3°C / h.

[0084] Example 8

[0085] A microporous low thermal conductivity composite silica brick, the thermal insulation layer is composed of the following raw materials in percentage by mass: 70% (less than 8 mm) of polyslightly porous siliceous homogenized material, 24% (less than 100 μm) of quartz powder, 3% (less than 10 μm) of silicon powder, 0.9% of sodium tripolyphosphate, 0.12% of sodium hexametaphosphate, 1.98% of binder II (aluminum dihydrogen phosphate), a total of 100%;

[0086] The working layer is composed of the following raw materials in percentage by mass: 52% silica sand (1.5-3.0 mm), 35% silica powder (less than 100 μm), 1% binder I (lignin, dextrin and phosphate in a mass ratio of 1:1:1), 5% fluorite powder (less than 100 μm), 7% silicon micropowder (less than 10 μm), 0% iron scale powder (less than 100 μm), and 0% calcium oxide, totaling 100%.

[0087] The method for preparing the above-mentioned microporous low thermal conductivity composite silica brick comprises the following steps:

[0088] Weigh the raw materials of the working layer and the thermal insulation layer, premix the raw materials of the working layer and the thermal insulation layer respectively to obtain a working layer premix and a thermal insulation layer premix, respectively load the working layer premix and the thermal insulation layer premix into molds, separate them with templates in the middle, remove the templates after filling, and then press at 130MPa for 8min, and then place in a 140°C drying kiln to dry until the moisture content is less than 2% to obtain a brick, the thickness ratio of the working layer and the thermal insulation layer is 2:1, heat the brick to 1400°C, keep warm for 13h, and cool with the furnace to obtain;

[0089] The heating procedure is: heating to 400°C at 20°C / h, heating to 600°C at 25°C / h, heating to 1200°C at 7°C / h, and heating to 1400°C at 1-3°C / h.

[0090] Example 9

[0091] A microporous low thermal conductivity composite silica brick, the thermal insulation layer is composed of the following raw materials in percentage by mass: 67% (less than 8mm) of polyslightly porous siliceous homogenized material, 25% (less than 100μm) of quartz powder, 6% (less than 10μm) of silicon powder, 0.5% of sodium tripolyphosphate, 0.3% of sodium hexametaphosphate, 1.2% of binder II (aluminum dihydrogen phosphate), a total of 100%;

[0092] The working layer is composed of the following raw materials in percentage by mass: 68% silica sand (1.5-3.0 mm), 15% silica powder (less than 100 μm), 2% binder I (lignin, cellulose and dextrin in a mass ratio of 1:1:1), 4% fluorite powder (less than 100 μm), 8% silicon micropowder (less than 10 μm), 0% iron scale powder (less than 100 μm), and 3% calcium oxide, totaling 100%.

[0093] The method for preparing the above-mentioned microporous low thermal conductivity composite silica brick comprises the following steps:

[0094] Weigh the raw materials of the working layer and the thermal insulation layer, premix the raw materials of the working layer and the thermal insulation layer respectively to obtain a working layer premix and a thermal insulation layer premix, respectively load the working layer premix and the thermal insulation layer premix into molds, separate them with templates, remove the templates after filling, press at 120MPa for 3min, and then place in a 150°C drying kiln to dry until the moisture is less than 2% to obtain a brick, the thickness ratio of the working layer to the thermal insulation layer is 3:1.2, heat the brick to 1450°C, keep warm for 13h, and cool with the furnace to obtain;

[0095] The heating procedure is: heating to 200°C at 20°C / h, heating to 1100°C at 25°C / h, heating to 1300°C at 7°C / h, and heating to 1450°C at 1-3°C / h.

[0096] Example 10

[0097] A microporous low thermal conductivity composite silica brick, the thermal insulation layer is composed of the following raw materials in percentage by mass: 73% (less than 8 mm) of polymicroporous siliceous homogenized material, 23% (less than 100 μm) of quartz powder, 2% (less than 10 μm) of silicon powder, 0.6% of sodium tripolyphosphate, 0.1% of sodium hexametaphosphate, 1.3% of binder II (aluminum dihydrogen phosphate), a total of 100%;

[0098] The working layer is composed of the following raw materials in percentage by mass: 60% silica sand (1.5-3.0 mm), 25% silica powder (less than 100 μm), 1% binder I (lignin, cellulose, dextrin and phosphate in a mass ratio of 1:1:1:1), 2.5% fluorite powder (less than 100 μm), 10% silicon micropowder (less than 10 μm), 1.5% iron scale powder (less than 100 μm), and 0% calcium oxide, totaling 100%.

[0099] The method for preparing the above-mentioned microporous low thermal conductivity composite silica brick comprises the following steps:

[0100] Weigh the raw materials of the working layer and the thermal insulation layer, premix the raw materials of the working layer and the thermal insulation layer respectively to obtain a working layer premix and a thermal insulation layer premix, respectively load the working layer premix and the thermal insulation layer premix into molds, separate them with templates, remove the templates after filling, press at 150MPa for 8min, and then place in a 180°C drying kiln to dry until the moisture is less than 2% to obtain a brick, the thickness ratio of the working layer to the thermal insulation layer is 4:0.8, heat the brick to 1380°C, keep warm for 12h, and cool with the furnace to obtain;

[0101] The heating procedure is: heating to 500°C at 20°C / h, heating to 1000°C at 25°C / h, heating to 1200°C at 7°C / h, and heating to 1300°C at 1-3°C / h.

[0102] The mechanical strength and thermal insulation performance of the microporous low thermal conductivity composite silica bricks prepared in the above Examples 1 to 10 were tested, and the results are shown in Table 1 below. Since the performance of the microporous low thermal conductivity composite silica bricks prepared in Examples 1 to 10 are similar, only Examples 1, 3, 5, 7 and 10 are used as examples to illustrate the effects.

[0103] Table 1 Mechanical strength and thermal insulation performance of the microporous low thermal conductivity composite silicon brick of the present invention

[0104]

[0105]

[0106] It can be seen from Table 1 that the mechanical strength and thermal insulation performance of the microporous low thermal conductivity composite silica brick prepared by the present invention are both good. Increasing the proportion of the poly-microporous siliceous homogenizing material is beneficial to the improvement of the compressive strength and load softening temperature of the composite silica brick, but it will also increase the porosity accordingly. The thermal conductivity shows a trend of first decreasing and then increasing with the increase of the content of the poly-microporous siliceous homogenizing material. Increasing the molding pressure can increase the compressive strength of the composite silica brick and reduce the porosity, but when the pressure increases to a certain extent, the thermal conductivity will increase accordingly.

[0107] In summary, the thermal insulation layer used in the present invention is formed by combining 65% to 75% by mass of slightly porous siliceous homogenized material, 20% to 25% quartz powder, 2% to 8% silicon powder, 0.1% to 1% sodium tripolyphosphate, 0.05% to 0.3% sodium hexametaphosphate and 1% to 2% binder II. The working layer has the high strength of traditional silica bricks, directly contacts high-temperature materials, has high-temperature wear resistance, high load softening temperature, corrosion resistance, and thermal shock resistance, achieving stable and long-life use effects; the thermal insulation layer adopts a special high-strength porous material, which has the characteristics of high strength, low thermal conductivity, good strength and thermal insulation effect, and energy saving and consumption reduction, thereby achieving the high strength and thermal insulation effect of the composite silica brick.

[0108] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A microporous low thermal conductivity composite silica brick, comprising a working layer and a thermal insulation layer, wherein the thermal insulation layer is wrapped outside the working layer; characterized in that: The thickness ratio of the working layer to the insulation layer is 2-4:0.6-1.2; The thermal insulation layer is composed of the following raw materials in percentage by mass: 65% to 75% of polyslightly porous siliceous homogenizing material, 20% to 25% of quartz powder, 2% to 8% of silicon powder, 0.1% to 1% of sodium tripolyphosphate, 0.05% to 0.3% of sodium hexametaphosphate, and 1% to 2% of binder II, totaling 100%.

2. The microporous low thermal conductivity composite silica brick according to claim 1, characterized in that: The thickness ratio of the working layer to the thermal insulation layer is 2 to 4:

1.

3. The microporous low thermal conductivity composite silica brick according to claim 1, characterized in that: The binder II is phosphoric acid or a phosphate binder.

4. The microporous low thermal conductivity composite silica brick according to claim 1, characterized in that: The working layer is composed of the following raw materials in percentage by mass: 50% to 70% silica sand, 15% to 35% silica powder, 1% to 2.5% binder I, 2% to 5% fluorite powder, 5% to 10% silicon micropowder, 0% to 1.5% iron scale powder, and 0% to 3% calcium oxide, which totals 100%.

5. The microporous low thermal conductivity composite silica brick according to claim 4, characterized in that: The binder I is one or more of lignin, cellulose, dextrin and phosphate.

6. A method for preparing the microporous low thermal conductivity composite silica brick according to any one of claims 1 to 5, characterized in that: The following steps are involved: Weigh the raw materials of the working layer and the insulation layer respectively; Mix 50% to 70% by mass of silica sand, 15% to 35% of silica powder, 1% to 2.5% of binder I, 2% to 5% of fluorite powder, 5% to 10% of silicon micropowder, 0% to 1.5% of iron scale powder, and 0% to 3% of calcium oxide to obtain a working layer premix; Mix 65% to 75% by mass of slightly porous siliceous homogenized material, 20% to 25% of quartz powder, 2% to 8% of silicon powder, 0.1% to 1% of sodium tripolyphosphate, 0.05% to 0.3% of sodium hexametaphosphate, and 1% to 2% of binder II to obtain a premix for the thermal insulation layer; The working layer premix and the insulation layer premix are pressed into shape and dried to obtain a brick blank, and the brick blank is heated to 1300-1450° C., kept warm, and cooled to obtain the brick blank.

7. The preparation method according to claim 6, characterized in that: During pressing, the pressure is 100-150 MPa and the time is 3-10 minutes.

8. The preparation method according to claim 6, characterized in that: The insulation time is 5 to 15 hours.

9. The preparation method according to claim 6, characterized in that: The heating procedure is: heating to 200-600°C at 20°C / h, heating to 600-1100°C at 25°C / h, heating to 1100-1350°C at 7°C / h, and heating to 1300-1450°C at 1-3°C / h.

10. The preparation method according to claim 6, characterized in that: During drying, the bricks are dried in a drying kiln at 100-200°C to obtain bricks with a moisture content of less than 2%.

Citation Information

Patent Citations

  • Silicon corundum wearproof composite brick

    CN106938923A

  • Lightweight high-strength layered refractory material and preparation method thereof

    CN116375484A

  • Preparation method of lightweight high-aluminum poly-light brick

    CN117567144A

  • High-strength polylight mullite microporous castable and preparation method thereof

    CN118290170A

  • Preparation method of microporous high-strength light silicon homogenized material

    CN118307332A