Microporous low-thermal-conductivity composite mullite brick and preparation method thereof

By using microporous low-thermal conductivity composite mullite bricks in high-temperature equipment, combining high-quality aluminum-silicon raw materials and polylight mullite microporous homogenization materials, the problems of low strength and poor thermal insulation effect of traditional thermal insulation materials are solved. It achieves high strength and good thermal insulation performance, extends the service life of the equipment and saves energy and reduces consumption.

CN118993716APending Publication Date: 2024-11-22WUHAN UNIV OF SCI & TECH +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411078665.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Traditional thermal insulation materials have low strength and poor thermal insulation effect in high-temperature equipment, making it difficult to combine well with lining bricks, resulting in heat loss and equipment damage.

Method used

Using microporous low-thermal conductivity composite mullite bricks, the use of high-quality aluminum-silicon raw materials and independently developed polylight mullite microporous homogenizers in the working layer and insulation layer, combining calcium aluminate cement, silicon micropowder and high Aluminum fine powder forms multi-layer structural bricks, improving strength and thermal insulation performance.

Benefits of technology

It realizes high strength and good thermal insulation performance of high-temperature equipment, is suitable for fixed and relatively moving equipment, extends the service life of the equipment, and achieves energy saving and consumption reduction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993716A_ABST
    Figure CN118993716A_ABST
Patent Text Reader

Abstract

The invention discloses a microporous low-thermal-conductivity composite mullite brick and a preparation method thereof, and belongs to the technical field of mullite bricks, the prepared composite mullite brick is formed by compounding a plurality of layers of structures, and has high strength and good thermal insulation performance. Wherein the working layer is prepared from high-quality aluminum-silicon raw materials, and has the advantages of low heat conductivity coefficient, high heat stability, high refractoriness under load, high normal-temperature compression strength, stable chemical property, higher high-temperature wear resistance and certain alkali corrosion resistance; according to the thermal insulation layer, 50%-60% of independently researched and developed polylight mullite microporous homogenized material is adopted as a low-heat-conduction main component, 5%-10% of calcium aluminate cement and 3%-11% of silica powder are adopted as binding agents, 2%-10% of natural aluminum-silicon refractory raw material, 20%-30% of high-aluminum fine powder is adopted as an expansion regulator, and 1%-2% of a water reducing agent is adopted to improve the dispersion effect of the fine powder. And the prepared insulating layer has the characteristics of high bonding strength and low heat conductivity coefficient.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of mullite bricks, and in particular to a microporous low-thermal-conductivity composite mullite brick and a preparation method thereof. Background Art

[0002] Refractories are generally divided into two types: unshaped and shaped. Unshaped refractories, also known as castables, are a mixture of various aggregates or aggregates and one or more binders in a powdered form. They must be mixed with one or more liquids to ensure uniformity and high fluidity. Shaped refractories generally refer to refractory bricks, which have standard shapes but can also be temporarily fabricated as needed. Refractory bricks are made by firing refractory clay or other refractory raw materials. They are pale yellow or light brown and primarily used in smelting furnaces. They can withstand temperatures of 1580°C to 1770°C and have a specific shape and size. Based on the manufacturing process, they can be categorized into fired bricks, unfired bricks, fused bricks (cast bricks), and refractory insulating bricks. Based on shape and size, they can be divided into standard, ordinary, and specialized bricks. They are used as high-temperature building and structural materials in furnaces and various thermal equipment, and can withstand various physical, chemical, and mechanical changes at high temperatures. Such as refractory clay bricks, high alumina bricks, silica bricks, magnesia bricks, etc.

[0003] Existing refractory bricks and insulation bricks are all made of a single material. When used, bricks with multiple properties need to be used in combination. When used on relatively fixed equipment, the combination of rotating bricks with various properties can still meet the requirements. However, on some relatively moving equipment, such as rotary kilns, the combination of various bricks is difficult to meet the requirements. In particular, in the use of rotary kilns, insulation materials are used to reduce the temperature of the kiln shell. However, traditional insulation materials have low strength and poor insulation effect. They cannot be well combined with lining bricks and are easily damaged during operation, resulting in a large amount of heat loss and damage to the equipment. To this end, the present invention provides a microporous low thermal conductivity composite mullite brick and a preparation method thereof. Summary of the Invention

[0004] The present invention provides a microporous low thermal conductivity composite mullite brick and a preparation method thereof, which effectively solves the technical problems that traditional thermal insulation materials have low strength, poor thermal insulation effect, cannot be well combined with lining bricks, and are easily damaged during operation, thereby causing a large amount of heat loss and damage to equipment. At the same time, a preparation method of a microporous low thermal conductivity composite mullite brick is provided, which has both strength and thermal insulation performance, and can achieve energy saving and consumption reduction and extend the service life of high-temperature equipment.

[0005] The first object of the present invention is to provide a microporous low thermal conductivity composite mullite brick, comprising a working layer and an insulation layer, wherein the insulation layer is wrapped around the working layer, and wherein the thickness ratio of the working layer to the insulation layer is 2-4:0.5-1;

[0006] The thermal insulation layer is composed of the following raw materials in percentage by mass: 50% to 60% of poly-light mullite microporous homogenizing material, 5% to 10% of calcium aluminate cement, 3% to 11% of silicon micropowder, 2% to 10% of natural aluminum silicate refractory raw material, 20% to 30% of high aluminum fine powder, and 1% to 2% of water reducer, which totals 100%.

[0007] As a preferred embodiment, the natural aluminosilicate refractory raw material is one or more of andalusite, kyanite, and sillimanite.

[0008] As a preferred embodiment, the alumina content of the high-aluminum fine powder is 80% to 95%.

[0009] As a preferred embodiment, the working layer is composed of the following raw materials in the following mass percentages: 10% to 15% fused mullite, 48% to 56% homogenized alumina clinker, 3% to 8% silicon carbide, 10% to 16% andalusite, 6% to 11% binder, and 3% to 5% additives, totaling 100%.

[0010] As a preferred embodiment, the binder is phosphate or Guangxi white mud.

[0011] As a preferred embodiment, the additive is corundum powder or steel fiber.

[0012] The second object of the present invention is to provide a method for preparing the above-mentioned microporous low thermal conductivity composite mullite brick, which is characterized by comprising the following steps:

[0013] Weigh the raw materials of the working layer and the insulation layer respectively;

[0014] The working layer premix is ​​obtained by mixing 10% to 15% of fused mullite, 48% to 56% of homogenized alumina clinker, 3% to 8% of silicon carbide, 10% to 16% of andalusite, 6% to 11% of a binder, and 3% to 5% of an additive in percentage by mass.

[0015] The premix of the thermal insulation layer is obtained by mixing 50% to 60% by mass of poly-light mullite microporous homogenized material, 5% to 10% of calcium aluminate cement, 3% to 11% of silica powder, 2% to 10% of natural alumina-silica refractory raw material, 20% to 30% of high-alumina fine powder, and 1% to 2% of water reducer.

[0016] The working layer premix and the insulation layer premix are pressed and formed, and dried to obtain bricks. The bricks are heated to 1200-1500° C., kept warm, and cooled to obtain the bricks.

[0017] As a preferred embodiment, during pressing, the pressure is 120-180 MPa and the time is 5-15 minutes.

[0018] As a preferred embodiment, the insulation time is 3 to 24 hours.

[0019] As a preferred embodiment, the temperature is increased at 10-30°C / min to 1000°C, and then increased at 1-10°C / min to 1200-1500°C.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The present invention provides a microporous, low-thermal-conductivity composite mullite brick and its preparation method. The composite mullite brick prepared by the present invention is composed of a multi-layer composite structure and has both high strength and good thermal insulation performance. The working layer is prepared from high-quality aluminum-silica raw materials and has low thermal conductivity, high thermal stability, high refractoriness under load, high compressive strength at room temperature, stable chemical properties, high high-temperature wear resistance, and certain resistance to alkali corrosion. The thermal insulation layer uses 50% to 60% of independently developed polylight mullite microporous homogenizing material as the main low-thermal-conductivity component, 5% to 10% calcium aluminate cement and 3% to 11% silica powder as binders, 2% to 10% natural aluminum-silica refractory raw materials and 20% to 30% high-aluminum fine powder as expansion regulators, and 1% to 2% water reducer to improve the dispersion of micro- and fine powders. The prepared thermal insulation layer has the characteristics of high bonding strength and low thermal conductivity. The multi-layer composite mullite bricks formed by the present invention have high strength, enabling their use in both fixed high-temperature equipment and relatively moving equipment, such as rotary kilns, meeting the technical and operational requirements of high-temperature equipment. The present invention achieves energy conservation and consumption reduction, extending the service life of high-temperature equipment, and features a scientific preparation method and convenient construction. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a physical picture of the microporous low thermal conductivity composite mullite brick of the present invention. DETAILED DESCRIPTION

[0023] To enable those skilled in the art to better understand and implement the technical solutions of the present invention, the present invention is further described below with reference to specific examples and accompanying drawings. However, the examples are not intended to limit the present invention. The following experimental and detection methods are conventional methods unless otherwise specified; the reagents and raw materials are commercially available unless otherwise specified.

[0024] The background technology of the present invention mentioned that the existing refractory bricks and insulating bricks are all made of a single material structure. When used, bricks with multiple properties need to be used in combination. When used on relatively fixed equipment, the combination of rotary bricks with various properties can also meet the requirements. However, on some relatively moving equipment, such as rotary kilns, it is difficult to meet the requirements by using various bricks in combination. In particular, in the use of rotary kilns, in order to reduce the temperature of the kiln shell, thermal insulation materials are used. However, traditional thermal insulation materials have low strength and poor thermal insulation effect. They cannot be well combined with lining bricks and are easily damaged during operation, resulting in a large amount of heat loss and damage to the equipment. Based on the above technical problems, the present invention provides a microporous low thermal conductivity composite mullite brick and a preparation method thereof, wherein the working layer is prepared from high-quality aluminum-silica raw materials, and has the advantages of low thermal conductivity, high thermal stability, high load softening temperature, high compressive strength at room temperature, stable chemical properties, high high-temperature wear resistance and certain resistance to alkali corrosion. The insulation layer uses 50% to 60% of independently developed poly-light mullite microporous homogenized material as the main low-thermal conductivity component, 5% to 10% calcium aluminate cement and 3% to 11% silica powder as binders, 2% to 10% natural aluminum-silica refractory raw materials and 20% to 30% high-aluminum fine powder as expansion regulators, and 1% to 2% water reducer to improve the dispersion of the micro- and fine powders. The prepared insulation layer has the characteristics of high bonding strength and low thermal conductivity. The multi-layer composite mullite bricks finally formed by the present invention have high strength, making them suitable for use on both fixed high-temperature equipment and relatively moving equipment, such as rotary kilns, and can meet the technical and usage requirements of high-temperature equipment. The present invention achieves energy conservation and consumption reduction, extends the service life of high-temperature equipment, and has a scientific preparation method and convenient construction.

[0025] The technical solution of the present invention is analyzed and explained in detail below.

[0026] The present invention first provides a microporous low thermal conductivity composite mullite brick, comprising a working layer and a thermal insulation layer, wherein the thermal insulation layer is wrapped around the working layer, and the thickness ratio of the working layer to the thermal insulation layer is 2-4:0.5-1;

[0027] The thermal insulation layer is composed of the following raw materials in percentage by mass: 50% to 60% of poly-light mullite microporous homogenizer, 5% to 10% of calcium aluminate cement (Kenos Secar71, particle size less than 20 μm), 3% to 11% of silica micropowder (Aiken 95U-1, particle size less than 10 μm), 2% to 10% of natural aluminum silicate refractory raw material, 20% to 30% of high aluminum fine powder (particle size less than 45 μm), and 1% to 2% of water reducer, totaling 100%. The insulation layer uses 50% to 60% of the independently developed poly-light mullite microporous homogenized material as the main component with low thermal conductivity, 5% to 10% calcium aluminate cement and 3% to 11% silicon micropowder as binders, 2% to 10% natural aluminum silicate refractory raw materials and 20% to 30% high aluminum fine powder as expansion regulators, and 1% to 2% water reducer to improve the dispersion effect of micro and fine powders. The prepared insulation layer has the characteristics of high bonding strength and low thermal conductivity.

[0028] The working layer is composed of the following raw materials by mass: 10%-15% fused mullite, 48%-56% homogenized alumina clinker, 3%-8% silicon carbide, 10%-16% andalusite, 6%-11% binder, and 3%-5% additives, totaling 100%. The working layer is made from high-quality aluminosilicate raw materials and exhibits low thermal conductivity, high thermal stability, a high refractoriness under load, high compressive strength at room temperature, stable chemical properties, high high-temperature wear resistance, and a certain degree of resistance to alkali corrosion. The natural aluminosilicate refractory raw materials are one or more of andalusite, kyanite, and sillimanite.

[0029] It should be noted that the alumina content of the high-alumina fine powder is 80% to 95%. The natural alumina-silica refractory raw material and the high-alumina fine powder are used in conjunction with each other, and the total amount of the two is consistent. The type and amount of the natural alumina-silica refractory raw material used controls the expansion of the insulation material and ensures the material's volume stability at high temperatures.

[0030] In order to further achieve a good bonding effect between the components in the working layer of the present invention, the binder is phosphate or Guangxi white mud.

[0031] In order to further improve the mechanical strength of the microporous low thermal conductivity composite mullite brick, the additive is corundum powder or steel fiber.

[0032] The present invention also provides a method for preparing the above-mentioned microporous low thermal conductivity composite mullite brick, comprising the following steps:

[0033] Weigh the raw materials of the working layer and the insulation layer respectively;

[0034] The working layer premix is ​​obtained by mixing 10% to 15% of fused mullite, 48% to 56% of homogenized alumina clinker, 3% to 8% of silicon carbide, 10% to 16% of andalusite, 6% to 11% of a binder, and 3% to 5% of an additive in percentage by mass.

[0035] The premix of the thermal insulation layer is obtained by mixing 50% to 60% by mass of poly-light mullite microporous homogenized material, 5% to 10% of calcium aluminate cement, 3% to 11% of silica powder, 2% to 10% of natural alumina-silica refractory raw material, 20% to 30% of high-alumina fine powder, and 1% to 2% of water reducer.

[0036] The working layer premix and the insulation layer premix are pressed and formed, and dried to obtain bricks. The bricks are heated to 1200-1500° C., kept warm, and cooled to obtain the bricks.

[0037] In order to ensure a good bonding effect between the insulation layer and the working layer, the pressing pressure is 120-180 MPa and the pressing time is 5-15 minutes.

[0038] In order to improve the mechanical strength of the bricks during the firing process, the insulation time is 3 to 24 hours.

[0039] To minimize cracking in the thermal insulation and working layers of the bricks caused by transient temperature rise and silicon oxide crystal transformation during the brick firing process, the heating program is as follows: increasing the temperature to 1000°C at 10-30°C / min, and then increasing the temperature to 1200-1500°C at 1-10°C / min. This gradient heating method can minimize cracking in the bricks.

[0040] The effects are described below through specific examples and comparative examples.

[0041] Example 1

[0042] A microporous low thermal conductivity composite mullite brick, wherein the working layer is composed of the following raw materials in percentage by mass: 10% fused mullite, 56% homogenized alumina clinker, 3% silicon carbide, 16% andalusite, 10% binder (aluminum dihydrogen phosphate), and 5% additive (plate-shaped corundum fine powder with a particle size of 15 to 30 μm), totaling 100%.

[0043] The insulation layer is composed of the following raw materials in the following mass percentages: 50% poly-light mullite microporous homogenizer, 10% calcium aluminate cement (Kenos Secar71, particle size less than 20μm), 3% silica powder (Aiken 95U-1, particle size less than 10μm), 10% natural alumina-silica refractory raw material (andalusite), 26% high alumina fine powder (particle size less than 45μm), 1% water reducer (sodium tripolyphosphate), totaling 100%.

[0044] The preparation method of the above-mentioned microporous low thermal conductivity composite mullite brick comprises the following steps:

[0045] Weigh the raw materials of the working layer and the thermal insulation layer, premix the raw materials of the working layer and the thermal insulation layer respectively to obtain a working layer premix and a thermal insulation layer premix, respectively put the working layer premix and the thermal insulation layer premix into a mold, separate them with a template in the middle, remove the template after filling, and then press at 120 MPa for 5 minutes, dry to obtain a brick, the thickness ratio of the working layer to the thermal insulation layer is 2:0.5, heat the brick to 1200 ° C, keep warm for 24 hours, and cool with the furnace to obtain;

[0046] The temperature was raised to 1000° C. at 30° C. / min, and then raised to 1200° C. at 10° C. / min.

[0047] Example 2

[0048] A microporous low thermal conductivity composite mullite brick, wherein the working layer is composed of the following raw materials in percentage by mass: 15% fused mullite, 48% homogenized alumina clinker, 8% silicon carbide, 15% andalusite, 11% binder (aluminum dihydrogen phosphate), and 3% additive (plate-shaped corundum fine powder with a particle size of 15 to 30 μm), totaling 100%.

[0049] The insulation layer is composed of the following raw materials in the following mass percentages: 60% poly-light mullite microporous homogenizer, 5% calcium aluminate cement (Kenos Secar71, particle size less than 20μm), 11% silica powder (Aiken 95U-1, particle size less than 10μm), 2% natural alumina-silica refractory raw material (kyanite), 20% high alumina fine powder (particle size less than 45μm), and 2% water reducer (sodium tripolyphosphate), totaling 100%.

[0050] The preparation method of the above-mentioned microporous low thermal conductivity composite mullite brick comprises the following steps:

[0051] Weigh the raw materials of the working layer and the thermal insulation layer, premix the raw materials of the working layer and the thermal insulation layer respectively to obtain a working layer premix and a thermal insulation layer premix, respectively load the working layer premix and the thermal insulation layer premix into a mold, separate them with a template in the middle, remove the template after filling, and then press at 160 MPa for 10 minutes, dry to obtain a brick, the thickness ratio of the working layer to the thermal insulation layer is 2:1, heat the brick to 1400 ° C, keep warm for 10 hours, and cool with the furnace to obtain;

[0052] The temperature was raised to 1000° C. at 20° C. / min, and then raised to 1400° C. at 1° C. / min.

[0053] Example 3

[0054] A microporous low thermal conductivity composite mullite brick, wherein the working layer is composed of the following raw materials in percentage by mass: 15% fused mullite, 54% homogenized alumina clinker, 7% silicon carbide, 14% andalusite, 6% binder (aluminum dihydrogen phosphate), and 4% additive (plate-shaped corundum fine powder with a particle size of 15 to 30 μm), totaling 100%.

[0055] The insulation layer is composed of the following raw materials in the following mass percentages: 53% poly-light mullite microporous homogenizer, 6% calcium aluminate cement (Kenos Secar71, particle size less than 20μm), 5% silica micropowder (Aiken 95U-1, particle size less than 10μm), 5% natural alumina-silica refractory raw material (sillimanite), 30% high alumina fine powder (particle size less than 45μm), 1% water reducer (sodium tripolyphosphate), totaling 100%.

[0056] The preparation method of the above-mentioned microporous low thermal conductivity composite mullite brick comprises the following steps:

[0057] Weigh the raw materials of the working layer and the thermal insulation layer, premix the raw materials of the working layer and the thermal insulation layer respectively to obtain a working layer premix and a thermal insulation layer premix, respectively put the working layer premix and the thermal insulation layer premix into a mold, separate them with a template in the middle, remove the template after filling, and then press at 180 MPa for 15 minutes, dry to obtain a brick, the thickness ratio of the working layer to the thermal insulation layer is 4:0.5, heat the brick to 1300 ° C, keep warm for 3 hours, and cool with the furnace to obtain;

[0058] The temperature was raised to 1000° C. at 10° C. / min, and then raised to 1300° C. at 5° C. / min.

[0059] Example 4

[0060] A microporous low thermal conductivity composite mullite brick, wherein the working layer is composed of the following raw materials in percentage by mass: 14% fused mullite, 56% homogenized alumina clinker, 7% silicon carbide, 10% andalusite, 8% binder (aluminum dihydrogen phosphate), and 5% additive (plate-shaped corundum fine powder with a particle size of 15 to 30 μm), totaling 100%.

[0061] The insulation layer is composed of the following raw materials in the following mass percentages: 56% poly-light mullite microporous homogenized material, 8% calcium aluminate cement (Kenos Secar71, particle size less than 20μm), 8% silica powder (Aiken 95U-1, particle size less than 10μm), 6% natural alumina-silica refractory raw materials (sillimanite and kyanite with a mass ratio of 1:1), 21% high alumina fine powder (particle size less than 45μm), 1% water reducer (sodium tripolyphosphate), totaling 100%.

[0062] The preparation method of the above-mentioned microporous low thermal conductivity composite mullite brick comprises the following steps:

[0063] Weigh the raw materials of the working layer and the thermal insulation layer, premix the raw materials of the working layer and the thermal insulation layer respectively to obtain a working layer premix and a thermal insulation layer premix, respectively load the working layer premix and the thermal insulation layer premix into a mold, separate them with a template in the middle, remove the template after filling, and then press at 140 MPa for 8 minutes, dry to obtain a brick, the thickness ratio of the working layer to the thermal insulation layer is 4:1, heat the brick to 1500 ° C, keep warm for 12 hours, and cool with the furnace to obtain;

[0064] The heating procedure is: heating to 1000° C. at 10-30° C. / min, and then heating to 1500° C. at 1-10° C. / min.

[0065] Example 5

[0066] A microporous low thermal conductivity composite mullite brick, wherein the working layer is composed of the following raw materials in percentage by mass: 13% fused mullite, 52% homogenized alumina clinker, 6% silicon carbide, 16% andalusite, 9% binder (aluminum dihydrogen phosphate), and 4% additive (plate-shaped corundum fine powder with a particle size of 15 to 30 μm), totaling 100%.

[0067] The insulation layer is composed of the following raw materials in the following mass percentages: 50% poly-light mullite microporous homogenizer, 10% calcium aluminate cement (Kenos Secar71, particle size less than 20μm), 6% silica powder (Aiken 95U-1, particle size less than 10μm), 8% natural alumina-silica refractory raw materials (kyanite and sillimanite in a mass ratio of 1:1), 24% high alumina fine powder (particle size less than 45μm), and 2% water reducer (sodium tripolyphosphate), totaling 100%.

[0068] The preparation method of the above-mentioned microporous low thermal conductivity composite mullite brick comprises the following steps:

[0069] Weigh the raw materials of the working layer and the thermal insulation layer, premix the raw materials of the working layer and the thermal insulation layer respectively to obtain a working layer premix and a thermal insulation layer premix, respectively load the working layer premix and the thermal insulation layer premix into a mold, separate them with a template in the middle, remove the template after filling, and then press at 130 MPa for 12 minutes, dry to obtain a brick, the thickness ratio of the working layer to the thermal insulation layer is 3:1, heat the brick to 1300 ° C, keep warm for 14 hours, and cool with the furnace to obtain;

[0070] The temperature was raised to 1000° C. at 25° C. / min, and then raised to 1300° C. at 5° C. / min.

[0071] Example 6

[0072] A microporous low thermal conductivity composite mullite brick, wherein the working layer is composed of the following raw materials in percentage by mass: 12% fused mullite, 50% homogenized alumina clinker, 8% silicon carbide, 15% andalusite, 10% binder (aluminum dihydrogen phosphate), and 5% additive (plate-shaped corundum fine powder with a particle size of 15 to 30 μm), totaling 100%.

[0073] The insulation layer is composed of the following raw materials in the following mass percentages: 58% poly-light mullite microporous homogenized material, 7% calcium aluminate cement (Kenos Secar71, particle size less than 20μm), 4% silica micropowder (Aiken 95U-1, particle size less than 10μm), 4% natural alumina-silica refractory raw material (andalusite and sillimanite in a mass ratio of 1:1), 25% high-alumina fine powder (particle size less than 45μm), and 2% water reducer (sodium tripolyphosphate), totaling 100%.

[0074] The preparation method of the above-mentioned microporous low thermal conductivity composite mullite brick comprises the following steps:

[0075] Weigh the raw materials of the working layer and the thermal insulation layer, premix the raw materials of the working layer and the thermal insulation layer respectively to obtain a working layer premix and a thermal insulation layer premix, respectively load the working layer premix and the thermal insulation layer premix into a mold, separate them with a template in the middle, remove the template after filling, and then press at 170 MPa for 10 minutes, dry to obtain a brick, wherein the thickness ratio of the working layer to the thermal insulation layer is 3:0.5, heat the brick to 1200°C, keep warm for 18 hours, and cool with the furnace to obtain;

[0076] The temperature was raised to 1000° C. at 20° C. / min, and then raised to 1200° C. at 1° C. / min.

[0077] Example 7

[0078] A microporous low thermal conductivity composite mullite brick, wherein the working layer is composed of the following raw materials in percentage by mass: 14% fused mullite, 56% homogenized alumina clinker, 6% silicon carbide, 13% andalusite, 8% binder (aluminum dihydrogen phosphate), and 3% additive (plate-shaped corundum fine powder with a particle size of 15 to 30 μm), totaling 100%.

[0079] The insulation layer is composed of the following raw materials in the following mass percentages: 52% of polylight mullite microporous homogenized material, 9% of calcium aluminate cement (Kenos Secar71, particle size less than 20μm), 9% of silica micropowder (Aiken 95U-1, particle size less than 10μm), 3% of natural alumina-silica refractory raw materials (sillimanite, kyanite and sillimanite in a mass ratio of 1:1:1), 26% of high-alumina fine powder (particle size less than 45μm), and 1% of water reducer (sodium tripolyphosphate), totaling 100%.

[0080] The preparation method of the above-mentioned microporous low thermal conductivity composite mullite brick comprises the following steps:

[0081] Weigh the raw materials of the working layer and the thermal insulation layer, premix the raw materials of the working layer and the thermal insulation layer respectively to obtain a working layer premix and a thermal insulation layer premix, respectively load the working layer premix and the thermal insulation layer premix into a mold, separate them with a template in the middle, remove the template after filling, and then press at 150 MPa for 15 minutes, dry to obtain a brick, the thickness ratio of the working layer to the thermal insulation layer is 2:0.8, heat the brick to 1500 ° C, keep warm for 20 hours, and cool with the furnace to obtain;

[0082] The temperature was raised to 1000° C. at 30° C. / min, and then raised to 1500° C. at 5° C. / min.

[0083] Example 8

[0084] A microporous low thermal conductivity composite mullite brick, wherein the working layer is composed of the following raw materials in percentage by mass: 15% fused mullite, 50% homogenized alumina clinker, 5% silicon carbide, 14% andalusite, 11% binder (aluminum dihydrogen phosphate), and 5% additive (plate-shaped corundum fine powder with a particle size of 15 to 30 μm), totaling 100%.

[0085] The insulation layer is composed of the following raw materials in the following mass percentages: 54% poly-light mullite microporous homogenized material, 7% calcium aluminate cement (Kenos Secar71, particle size less than 20μm), 7% silica micropowder (Aiken 95U-1, particle size less than 10μm), 9% natural alumina-silica refractory raw materials (andalusite, kyanite and sillimanite in a mass ratio of 1:1:1), 21% high alumina fine powder (particle size less than 45μm), 2% water reducer (sodium tripolyphosphate), totaling 100%.

[0086] The preparation method of the above-mentioned microporous low thermal conductivity composite mullite brick comprises the following steps:

[0087] Weigh the raw materials of the working layer and the thermal insulation layer, premix the raw materials of the working layer and the thermal insulation layer respectively to obtain a working layer premix and a thermal insulation layer premix, respectively load the working layer premix and the thermal insulation layer premix into a mold, separate them with a template in the middle, remove the template after filling, and then press at 135 MPa for 5 minutes, dry to obtain a brick, the thickness ratio of the working layer to the thermal insulation layer is 4:0.8, heat the brick to 1400 ° C, keep warm for 16 hours, and cool with the furnace to obtain;

[0088] The temperature was raised to 1000° C. at a rate of 10° C. / min, and then raised to 1400° C. at a rate of 10° C. / min.

[0089] Example 9

[0090] A microporous low thermal conductivity composite mullite brick, wherein the working layer is composed of the following raw materials in percentage by mass: 11% fused mullite, 55% homogenized alumina clinker, 4% silicon carbide, 14% andalusite, 13% binder (aluminum dihydrogen phosphate), and 3% additive (plate-shaped corundum fine powder with a particle size of 15 to 30 μm), totaling 100%.

[0091] The insulation layer is composed of the following raw materials in the following mass percentages: 50% poly-light mullite microporous homogenized material, 5% calcium aluminate cement (Kenos Secar71, particle size less than 20μm), 10% silica micropowder (Aiken 95U-1, particle size less than 10μm), 9% natural alumina-silica refractory raw materials (andalusite, kyanite and sillimanite in a mass ratio of 1:1:1), 25% high alumina fine powder (particle size less than 45μm), 1% water reducer (sodium tripolyphosphate), totaling 100%.

[0092] The preparation method of the above-mentioned microporous low thermal conductivity composite mullite brick comprises the following steps:

[0093] Weigh the raw materials of the working layer and the thermal insulation layer, premix the raw materials of the working layer and the thermal insulation layer respectively to obtain a working layer premix and a thermal insulation layer premix, respectively load the working layer premix and the thermal insulation layer premix into a mold, separate them with a template in the middle, remove the template after filling, and then press at 175 MPa for 8 minutes, dry to obtain a brick, wherein the thickness ratio of the working layer to the thermal insulation layer is 3:0.6, heat the brick to 1300°C, keep warm for 6 hours, and cool with the furnace to obtain;

[0094] The temperature was raised to 1000° C. at 20° C. / min, and then raised to 1300° C. at 1° C. / min.

[0095] Example 10

[0096] A microporous low thermal conductivity composite mullite brick, wherein the working layer is composed of the following raw materials in percentage by mass: 12% fused mullite, 54% homogenized alumina clinker, 8% silicon carbide, 12% andalusite, 10% binder (aluminum dihydrogen phosphate), and 4% additive (plate-shaped corundum fine powder with a particle size of 15 to 30 μm), totaling 100%.

[0097] The insulation layer is composed of the following raw materials in the following mass percentages: 60% poly-light mullite microporous homogenizer, 10% calcium aluminate cement (Kenos Secar71, particle size less than 20μm), 4% silica powder (Aiken 95U-1, particle size less than 10μm), 3% natural alumina-silica refractory raw materials (andalusite, kyanite and sillimanite in a mass ratio of 1:1:1), 21% high-alumina fine powder (particle size less than 45μm), and 2% water reducer (sodium tripolyphosphate), totaling 100%.

[0098] The preparation method of the above-mentioned microporous low thermal conductivity composite mullite brick comprises the following steps:

[0099] Weigh the raw materials of the working layer and the thermal insulation layer, premix the raw materials of the working layer and the thermal insulation layer respectively to obtain a working layer premix and a thermal insulation layer premix, respectively put the working layer premix and the thermal insulation layer premix into a mold, separate them with a template in the middle, remove the template after filling, and then press at 160 MPa for 12 minutes, dry to obtain a brick, the thickness ratio of the working layer to the thermal insulation layer is 3:1, heat the brick to 1200 ° C, keep warm for 8 hours, and cool with the furnace to obtain;

[0100] The temperature was raised to 1000° C. at 10° C. / min, and then raised to 1200° C. at 5° C. / min.

[0101] The mechanical strength and thermal insulation performance of the microporous low thermal conductivity composite mullite bricks prepared in Examples 1 to 10 were tested, and the results are shown in Table 1 below. Since the performance of the microporous low thermal conductivity composite mullite bricks prepared in Examples 1 to 10 is similar, only Examples 2, 4, 5, 8 and 9 are used as examples to illustrate the effects.

[0102] Table 1 Mechanical strength and thermal insulation performance of the microporous low thermal conductivity composite mullite brick of the present invention

[0103]

[0104] As can be seen from Table 1, increasing the binder content in the working layer of the microporous low thermal conductivity composite mullite brick of the present invention is conducive to improving the strength, and its thermal shock stability decreases with decreasing the amount of silicon carbide added, and the introduction of andalusite can increase its refractoriness under load; the content of cement and silica powder in the thermal insulation layer plays a decisive role in its strength and apparent porosity. The higher the cement content, the higher the strength, the higher the silica powder content, the lower the apparent porosity, the introduction of natural alumina-silica refractory raw materials can increase its refractoriness under load, and the higher the content of poly-light mullite microporous homogenizing material, the lower its thermal conductivity and the better the thermal insulation effect.

[0105] In summary, the working layer of the microporous, low-thermal-conductivity composite mullite brick provided by the present invention is made from high-quality aluminosilicate raw materials and exhibits low thermal conductivity, high thermal shock stability, high refractoriness under load, high compressive strength at room temperature, stable chemical properties, high high-temperature wear resistance, and a certain degree of resistance to alkali corrosion. The insulation layer utilizes 50% to 60% of independently developed polylight mullite microporous homogenizer as the main low-thermal-conductivity component, 5% to 10% calcium aluminate cement, 3% to 11% silica powder as binders, 2% to 10% natural aluminosilicate refractory raw materials, 20% to 30% high-alumina fine powder as expansion regulators, and 1% to 2% water reducer to enhance the dispersion of the micro- and fine powders. The resulting insulation layer combines high bonding strength with low thermal conductivity.

[0106] Obviously, those skilled in the art may make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if such changes and modifications fall within the scope of the claims and their equivalents, the present invention is intended to include such changes and modifications.

Claims

1. A microporous low thermal conductivity composite mullite brick, comprising a working layer and an insulation layer, wherein the insulation layer is wrapped outside the working layer, characterized in that: The thickness ratio of the working layer to the insulation layer is 2-4:0.5-1; The thermal insulation layer is composed of the following raw materials in percentage by mass: 50% to 60% of polylight mullite microporous homogenizing material, 5% to 10% of calcium aluminate cement, 3% to 11% of silicon micropowder, 2% to 10% of natural aluminum silicate refractory raw material, 20% to 30% of high aluminum fine powder, and 1% to 2% of water reducing agent, which totals 100%.

2. The microporous low thermal conductivity composite mullite brick according to claim 1, characterized in that: The natural aluminosilicate refractory raw material is one or more of andalusite, kyanite and sillimanite.

3. The microporous low thermal conductivity composite mullite brick according to claim 1, characterized in that: The aluminum oxide content of the high aluminum fine powder is 80% to 95%.

4. The microporous low thermal conductivity composite mullite brick according to claim 1, characterized in that: The working layer is composed of the following raw materials in percentage by mass: 10% to 15% of fused mullite, 48% to 56% of homogenized alumina clinker, 3% to 8% of silicon carbide, 10% to 16% of andalusite, 6% to 11% of binder, and 3% to 5% of additives, which totals 100%.

5. The microporous low thermal conductivity composite mullite brick according to claim 4, characterized in that: The binder is phosphate or Guangxi white mud.

6. The microporous low thermal conductivity composite mullite brick according to claim 4, characterized in that: The additive is corundum powder or steel fiber.

7. A method for preparing the microporous low thermal conductivity composite mullite brick according to any one of claims 1 to 6, characterized in that: The following steps are involved: Weigh the raw materials of the working layer and the insulation layer respectively; Mix 10% to 15% by mass of fused mullite, 48% to 56% by mass of homogenized alumina clinker, 3% to 8% by mass of silicon carbide, 10% to 16% by mass of andalusite, 6% to 11% by mass of a binder, and 3% to 5% by mass of an additive to obtain a working layer premix; 50% to 60% by mass of poly-light mullite microporous homogenized material, 5% to 10% of calcium aluminate cement, 3% to 11% of silica powder, 2% to 10% of natural aluminum silicon refractory raw material, 20% to 30% of high aluminum fine powder, and 1% to 2% of water reducer are mixed to obtain a premix for the thermal insulation layer; The working layer premix and the insulation layer premix are pressed and formed, and dried to obtain a brick blank. The brick blank is heated to 1200-1500° C., kept warm, and cooled to obtain the brick blank.

8. The preparation method according to claim 7, characterized in that: During pressing, the pressure is 120-180 MPa and the time is 5-15 minutes.

9. The preparation method according to claim 7, characterized in that: The insulation time is 3 to 24 hours.

10. The preparation method according to claim 7, characterized in that: The temperature is increased at 10-30°C / min to 1000°C, and then increased at 1-10°C / min to 1200-1500°C.

Citation Information

Patent Citations

  • Large compound energy-saving refractory brick and production method thereof

    CN102659422A

  • Corundum mullite composite brick and preparation method thereof

    CN109650854A