Glycidyl methacrylate modified hollow microspheres as well as preparation method and application thereof
By blending modified hollow microspheres with natural rubber, the environmental pollution and high cost problems of traditional fillers are solved, the mechanical properties and production efficiency of composite materials are improved, and environmentally friendly and economical rubber preparation is achieved.
Patent Information
- Application Number
- CN202411195071.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-22
AI Technical Summary
In the existing technology, traditional fillers such as carbon black can enhance the performance of rubber but cause environmental pollution problems, while high-performance alternatives such as silica are expensive, which limits their widespread application. There is a lack of environmentally friendly and economical alternatives.
Hollow microspheres were modified with silane coupling agents KH550 and KH570, and glycidyl methacrylate-modified hollow microspheres were prepared by grafting glycidyl methacrylate, and then blended with natural rubber to form a composite material.
The modified hollow microspheres enhance the interfacial bonding force between themselves and the rubber matrix, thereby improving the mechanical properties and vulcanization rate of the composite material, reducing production costs, minimizing environmental pollution, and providing excellent thermal and sound insulation properties.
Smart Images

Figure CN118994505A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of rubber composite material production, and particularly relates to glycidyl methacrylate modified hollow microspheres, a preparation method and application thereof. Background Art
[0002] In the production and application of rubber, the selection of fillers is crucial to adjust and optimize the key properties of rubber. Although traditional fillers such as carbon black can effectively enhance the performance of rubber, they may cause environmental pollution problems. The high cost of producing high-performance substitutes such as white carbon black limits their widespread application. Therefore, there is an urgent need to develop an alternative filler that is both environmentally friendly and economical to achieve sustainable development of the rubber manufacturing process and effective control of production costs.
[0003] Hollow microspheres are hollow silicate materials made by sintering industrial waste materials such as coal gangue, diatomaceous earth, marble powder, fly ash, etc. Its unique composition and structure give hollow microspheres rich physical and chemical properties. The hollow structure has the characteristics of light weight, low thermal conductivity, good sound insulation, and good thermal stability. After blending with polymers, composite materials with excellent sound insulation, heat insulation and outstanding compression permanent deformation can be obtained. Therefore, hollow microspheres have important application prospects in materials science. Summary of the invention
[0004] In view of the problems existing in the prior art, the object of the present invention is to provide a glycidyl methacrylate modified hollow microsphere, a preparation method and application thereof.
[0005] In order to achieve the above object, the present invention adopts the following technical solution:
[0006] The invention discloses a hollow microsphere modified with glycidyl methacrylate. Glycidyl methacrylate is grafted onto the hollow microsphere by using a silane coupling agent. The silane coupling agent is at least one of KH550, KH560, KH570 and Si69.
[0007] The preparation method of the glycidyl methacrylate modified hollow microspheres comprises the following steps:
[0008] (1) adding a silane coupling agent to anhydrous ethanol to prepare an anhydrous ethanol solution of the silane coupling agent; placing the dried hollow microspheres into the anhydrous ethanol solution of the silane coupling agent, stirring at a speed of 600-700 rpm in a water bath at 60° C.-70° C. for 1-2 h; washing the obtained sample three times to remove the unreacted silane coupling agent, and drying for later use;
[0009] (2) The sample prepared in step (1) is added to DMF, and then glycidyl methacrylate is added dropwise to the above solution, and AIBN is added as an initiator, and then the mixed solution is stirred at a speed of 600-700 rpm in a water bath at 80° C.-85° C. for 4-5 hours; the obtained sample is repeatedly washed with acetone and methanol and thoroughly dried to obtain glycidyl methacrylate modified hollow microspheres.
[0010] Based on the above solution, the silane coupling agent is at least one of KH550 and KH570.
[0011] Application of glycidyl methacrylate modified hollow microspheres prepared by the above method in the preparation of hollow microsphere / natural rubber composite materials.
[0012] A hollow microsphere / natural rubber composite material uses glycidyl methacrylate modified hollow microspheres prepared by the above method as fillers.
[0013] On the basis of the above scheme, the hollow microsphere / natural rubber composite material is prepared from the following components in parts by mass: 100 parts of natural rubber, 20 parts of carbon black, 30 parts of glycidyl methacrylate modified hollow microspheres prepared by the above method, 4 parts of zinc oxide, 2 parts of stearic acid, 2.5 parts of antioxidant 4020, 5 parts of paraffin oil, 1.5 parts of sulfur, and 1.3 parts of accelerator CZ.
[0014] The preparation method of the hollow microsphere / natural rubber composite material comprises the following steps:
[0015] (1) NR, carbon black, hollow microspheres modified with glycidyl methacrylate, zinc oxide, stearic acid, antioxidant 4020, and paraffin oil are added to an internal mixer and mixed for 5-10 minutes. After the rubber is discharged and cooled to room temperature, sulfur and accelerator CZ are added and mixed on an open mixer. After mixing evenly, the mixture is cooled down;
[0016] (2) placing the rubber mixture obtained in step (1) into a flat vulcanizer for vulcanization to obtain a hollow microsphere / natural rubber composite material.
[0017] On the basis of the above scheme, the temperature of the internal mixer is set to 90° C. and the rotor speed is set to 80 r / min.
[0018] On the basis of the above scheme, the vulcanization is carried out at a temperature of 150° C., a pressure of 10 MPa, and a time of 1.3×Tc90.
[0019] Advantages of the technical solution of the present invention
[0020] The present invention uses silane coupling agents γ-aminopropyl triethoxysilane (KH550) and γ-methacryloxypropyl trimethoxysilane (KH570) as intermediate reaction platforms for glycidyl methacrylate (GMA) modified hollow microspheres (RiM01). In this process, GMA reacts with epoxy ring-opening reaction and free radical polymerization reaction with KH550 and KH570 respectively. Different NR / RiM01@GMA composite materials are prepared by mechanical blending. The research results show that the addition of GMA improves the interfacial bonding force between RiM01 and NR, and the vulcanization rate and crosslinking degree of the rubber composite material are improved, but KH570 as a reaction platform is the most obvious improvement. Compared with the composite material of unmodified RiM01, the rubber composite material modified by glycidyl methacrylate has better mechanical properties. At the same time, when KH570 is used as a reaction platform, the interaction between the filler and the matrix is the strongest, and the rubber composite material has the smallest rolling resistance and the best heat-oxidative aging resistance.
[0021] The present invention uses GMA-modified hollow microspheres as fillers, and the prepared hollow microsphere / natural rubber composite material has the following advantages: First, the rubber filler hollow microspheres used are fillers made from industrial by-products, which are naturally available and non-toxic, and can reduce the pollution to the environment caused during the preparation process. Second, hollow microspheres can be used as a substitute for silica resources. Compared with other fillers, hollow microspheres are cheaper and can reduce the cost of production. Third, the modified hollow microspheres further improve the interfacial bonding force with the rubber matrix and the mechanical properties of the rubber composite material through chemical reactions; fourth, the hollow microspheres are lightweight and have a small size, which can improve the density, thermal insulation or rheology of the material, and perform outstandingly in materials with lightweight and high strength requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 Surface morphology of unmodified hollow microspheres;
[0023] Figure 2 Surface morphology of hollow microspheres R-KH550@GMA modified with glycidyl methacrylate;
[0024] Figure 3 Surface morphology of hollow microspheres R-KH570@GMA modified with glycidyl methacrylate;
[0025] Figure 4 Storage modulus (G') determination results of different hollow microsphere / natural rubber composites;
[0026] Figure 5 Determination results of loss factor (tanδ) of different hollow microsphere / natural rubber composites. DETAILED DESCRIPTION
[0027] The terms used in the present invention, unless otherwise specified, generally have the meanings commonly understood by those of ordinary skill in the art. The present invention will be further described in detail below in conjunction with specific examples and with reference to data. The following examples are intended to illustrate the present invention and are not intended to limit the scope of the present invention in any way.
[0028] The experimental methods in the following examples, unless otherwise specified, are all conventional methods, and are performed according to the techniques or conditions described in the literature in the field or according to the product instructions. The materials, reagents, etc. used in the following examples, unless otherwise specified, can all be obtained from commercial channels.
[0029] In the following embodiments,
[0030] KH550: γ-aminopropyltriethoxysilane
[0031] KH560: γ-Glycidyloxypropyltrimethoxysilane
[0032] KH570: γ-(methacryloyloxy)propyltrimethoxysilane
[0033] Si69: Bis-[γ-(triethoxysilyl)propyl]tetrasulfide
[0034] Natural rubber (NR) is a natural polymer compound mainly composed of cis-1,4-polyisoprene. About 91% to 94% of its components are rubber hydrocarbons (cis-1,4-polyisoprene), and the remaining components include non-rubber substances such as proteins, fatty acids, ash, and sugars. Natural rubber is one of the most widely used general-purpose rubbers.
[0035] Hollow microspheres are hollow structure products made of silicate, and their main components include calcium oxide and silicon dioxide. The main components are shown in Table 1:
[0036] Table 1 Main components of hollow microspheres
[0037]
[0038]
[0039] Example 1
[0040] A glycidyl methacrylate modified hollow microsphere is prepared by the following method:
[0041] (1) KH550 was added to anhydrous ethanol solution to prepare a 5% KH550 anhydrous ethanol solution; 55 g of the dried hollow microspheres were placed in 500 mL of the 5% KH550 anhydrous ethanol solution, and stirred at 600 rpm in a 60°C water bath for 1 h. The obtained sample was washed three times to remove unreacted KH550, and then placed in an oven to dry for use, thereby obtaining sample R-KH550.
[0042] (2) Take 50g of R-KH550 prepared in step (1) and add it to 500mL DMF (N,N-dimethylformamide, analytical grade), then add glycidyl methacrylate (GMA) dropwise to the above solution, the amount of GMA added is 10% of the mass of DMF, and AIBN is added as an initiator, wherein the mass of AIBN is 0.5% of the mass of GMA; then stir the mixed solution at 600 rpm in a water bath at 80°C for 4 hours. After the obtained sample is repeatedly washed with acetone and methanol and thoroughly dried, glycidyl methacrylate modified hollow microspheres (R-KH550@GMA) are obtained. The surface morphology of the unmodified hollow microspheres is as follows: Figure 1 As shown in Figure 2, the surface morphology of hollow microspheres R-KH550@GMA modified with glycidyl methacrylate is shown in Figure 2. Figure 2 shown.
[0043] Example 2
[0044] A glycidyl methacrylate modified hollow microsphere is prepared by the following method:
[0045] (1) KH570 was added to anhydrous ethanol solution to prepare a 5% KH570 anhydrous ethanol solution; 55 g of the dried hollow microspheres were placed in 500 mL of the 5% KH570 anhydrous ethanol solution, and stirred at 600 rpm in a 60°C water bath for 1 h. The obtained sample was washed three times to remove unreacted KH570, and then placed in an oven to dry for use, thereby obtaining sample R-KH570.
[0046] (2) Take 50g of R-KH570 prepared in step (1) and add it to 500mL DMF (N,N-dimethylformamide, analytical grade), then add glycidyl methacrylate (GMA) dropwise to the above solution, the amount of GMA added is 10% of the mass of DMF, and AIBN is added as an initiator, wherein the mass of AIBN is 0.5% of the mass of GMA; then stir the mixed solution at 600 rpm in a water bath at 80°C for 4 hours. After the obtained sample is repeatedly washed with acetone and methanol and thoroughly dried, glycidyl methacrylate modified hollow microspheres (R-KH570@GMA) are obtained. The surface morphology of the glycidyl methacrylate modified hollow microspheres R-KH570@GMA is as shown in FIG. Figure 3 shown.
[0047] Example 3
[0048] A hollow microsphere / natural rubber composite material, using glycidyl methacrylate modified hollow microspheres R-KH550@GMA prepared by the method of Example 1 as filler. The specific preparation method is as follows:
[0049] (1) NR, carbon black, R-KH550@GMA, ZnO, stearic acid, antioxidant 4020, and paraffin oil were added to an internal mixer and mixed for 5-10 minutes. The temperature of the internal mixer was set to 90°C and the rotor speed was set to 80 r / min. After the rubber was discharged and cooled to room temperature, sulfur and accelerator CZ were added to the open mixer and mixed. After mixing evenly, the sheet was cooled;
[0050] (2) placing the rubber mixture obtained in step (1) into a flat vulcanizer for vulcanization, setting the temperature to 150° C., the pressure to 10 MPa, and the vulcanization time to 1.3×Tc90; cooling at room temperature for 8-10 h after the vulcanization is completed, and obtaining a hollow microsphere / natural rubber composite material reinforced with R-KH550@GMA.
[0051] The formula of hollow microsphere / natural rubber composite material is shown in Table 2.
[0052] Table 2 Formulation of hollow microsphere / natural rubber composite materials
[0053]
[0054] Example 4
[0055] A hollow microsphere / natural rubber composite material, using the glycidyl methacrylate modified hollow microsphere R-KH570@GMA prepared by the method of Example 2 as a filler. Except that the filler is R-KH570@GMA, the other components and amounts are the same as those in Example 3, and the preparation method is the same as that in Example 3. That is, a hollow microsphere / natural rubber composite material reinforced with R-KH570@GMA is obtained.
[0056] Example 5
[0057] A hollow microsphere / natural rubber composite material, using the R-KH550 prepared in Example 1 as a filler. The remaining components and amounts are the same as those in Example 3, and the preparation method is the same as that in Example 3. Thus, a hollow microsphere / natural rubber composite material reinforced with R-KH550 is obtained.
[0058] Example 6
[0059] A hollow microsphere / natural rubber composite material, using the R-KH570 prepared in Example 2 as a filler. The remaining components and amounts are the same as those in Example 3, and the preparation method is the same as that in Example 3. Thus, a hollow microsphere / natural rubber composite material reinforced with R-KH570 is obtained.
[0060] Example 7
[0061] A hollow microsphere / natural rubber composite material uses R-KH560 (preparation method is the same as R-KH550) as filler. The remaining components and amounts are the same as those in Example 3, and the preparation method is the same as that in Example 3. Thus, a hollow microsphere / natural rubber composite material reinforced with R-KH560 is obtained.
[0062] Example 8
[0063] A hollow microsphere / natural rubber composite material uses R-Si69 (preparation method is the same as R-KH550) as filler. The remaining components and amounts are the same as those in Example 3, and the preparation method is the same as that in Example 3. Thus, a hollow microsphere / natural rubber composite material reinforced with R-Si69 is obtained.
[0064] Comparative Example
[0065] A hollow microsphere / natural rubber composite material uses unmodified hollow microspheres as fillers, and the remaining components and amounts are the same as those in Example 3, and the preparation method is the same as that in Example 3. Thus, a hollow microsphere / natural rubber composite material reinforced with unmodified hollow microspheres is obtained.
[0066] 1. Performance test of hollow microsphere / natural rubber composites
[0067] The curing time and scorch time of the hollow microsphere / natural rubber composite materials prepared by the methods described in Examples 3-8 and Comparative Examples were measured by a rotorless vulcanizer, the tensile strength and tear strength of the hollow microsphere / natural rubber composite materials prepared by the methods described in Examples 3-8 and Comparative Examples were measured by an electronic universal tensile testing machine, and the DIN abrasion tester was used to measure the DIN abrasion of the hollow microsphere / natural rubber composite materials prepared by the methods described in Examples 3-8 and Comparative Examples. The results are shown in Table 3.
[0068] Table 3 Performance test of hollow microsphere / natural rubber composites
[0069]
[0070] As shown in Table 3, the GMA molecular chain can effectively form an entangled structure with the rubber molecular chain and restrict the movement of the rubber molecular chain, thereby increasing the crosslinking density of the composite material and improving its physical and mechanical properties. In addition, the introduction of GMA into the composite material can also promote the vulcanization reaction of the composite material. As shown in Table 3, compared with the unmodified hollow microspheres, the vulcanization time (Tc90) of the composite material gradually decreases with the addition of GMA. This shows that the production efficiency of the composite material has been improved. This is attributed to the increase in active functional groups on the surface of the hollow microspheres after modification, which is easy to react with other substances, further promoting the vulcanization reaction of the rubber. The scorch time (Tc10) of the composite material did not change significantly. This result shows that even when GMA is introduced, the scorch time can remain stable, indicating that the processing safety of the composite material is basically the same. After the secondary modification of the hollow microspheres, the performance of the composite material is improved, indicating that the interface bonding force between the filler and the rubber is increased. This is because after GMA modification, epoxy groups and carbon-carbon double bonds exist on the surface of the hollow microspheres, which increases the entanglement between the filler and the rubber. This entanglement can dissipate more energy when the rubber is stressed, thus making the rubber composite material have better mechanical properties. Among them, compared with the unmodified hollow microspheres, the tensile strength of RiM01 treated with KH550 as a reaction platform has increased most significantly, by 24%; the tear strength and wear resistance of the hollow microspheres treated with KH570 as a reaction platform have increased most significantly, by 10% and 12% respectively.
[0071] The crosslinking degree of the hollow microsphere / natural rubber composite material prepared by the method described in Examples 3-8 and the comparative example was measured by a rotorless vulcanizer. The hollow microsphere / natural rubber composite material prepared by the method described in Examples 3-8 and the comparative example was aged by a hot oxygen aging box, and then the tensile strength and elongation at break of the hollow microsphere / natural rubber composite material prepared by the method described in Examples 3-8 and the comparative example after aging were measured by an electronic universal tensile machine. The results are shown in Table 4.
[0072] Table 4 Crosslinking degree and thermal oxidation aging resistance of hollow microsphere / natural rubber composites
[0073]
[0074] As shown in Table 4, the relationship between the maximum torque (MH) and the minimum torque (ML), MH-ML, is an important parameter reflecting the degree of crosslinking of the composite material. As can be seen from Table 4, after modification with silane coupling agents KH550 and KH570, MH-ML showed an upward trend. After secondary modification with GMA, it was further enhanced compared with the modification with silane coupling agent. This is because the GMA molecular chains on the surface of RiM01 show good compatibility with rubber and are entangled with each other, increasing the crosslinking density of the rubber. Oxygen affects natural rubber slowly at room temperature, but once heat is added, it accelerates the reaction with oxygen, resulting in rubber aging. Aging refers to the phenomenon that rubber materials gradually lose their ideal properties during storage or use, which also includes synthetic rubber. Rubber aging retention refers to the degree to which rubber is retained relative to its initial state after a certain aging process. Table 4 shows the tensile strength retention and elongation at break after aging of different rubber composites. After aging treatment, the mechanical properties of different rubber composites decreased to varying degrees. This is because the thermal oxidation aging caused the double bonds in the rubber molecular chain to break, resulting in a decrease in molecular weight, and the cross-linking ripening reaction caused the polysulfide bonds to be converted into disulfide bonds and monosulfide bonds, which may also have led to a decrease in fracture strain. The tensile strength retention and elongation at break of the hollow microsphere / natural rubber composites reinforced with R-KH550@GMA and R-KH570@GMA are higher than those of other materials.
[0075] 2. Dynamic Mechanical Properties
[0076] (1) Storage modulus (G') and loss factor (tanδ) test
[0077] The hollow microsphere / natural rubber composites prepared by the methods described in Examples 3-4 and Comparative Examples were tested using RPA (dynamic mechanical analyzer) to determine their storage modulus (G') and analyze the "Payne effect" in the material. These data can reflect the interaction strength between the filler and the matrix.
[0078] The results are as follows Figure 4 As shown, the variation of storage modulus (G') of different composite materials can be observed. Figure 4 It can be seen that with the silanization of hollow microspheres, the initial storage modulus of the composite material increases, and the initial storage modulus increases further after secondary grafting with GMA, which indicates that the interaction between the hollow microspheres and the rubber matrix is enhanced after modification. This is because after the modification treatment with silane coupling agent and GMA, a denser filling network is formed between the rubber and the filler. This denser filling network can enhance the interfacial interaction between the filler and the matrix, resulting in an increase in the initial value of the storage modulus.
[0079] pass Figure 5It can be observed that at low strain, the filler-filler network is hardly destroyed, and the energy dissipation mainly comes from the viscosity of the macromolecular chain. As the strain increases, friction becomes the main cause of energy dissipation, and the tanδ value gradually increases. The modified hollow microspheres have a lower tanδ value because the addition of GMA enhances the strength of the filled rubber network and limits the mobility of the rubber chain.
[0080] In the tire industry, the tanδ value is closely related to the rolling resistance of rubber composites, especially at a strain of 7%. Table 5 summarizes the tanδ values of different rubber composites at a strain of 7%. It can be seen from the table that the modified RiM01 can reduce the rolling resistance, among which KH570 has the most significant effect as a secondary reaction platform.
[0081] Table 5 Tanδ values of different composites at 7% strain
[0082]
[0083] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.
Claims
1. A glycidyl methacrylate modified hollow microsphere, characterized in that: The glycidyl methacrylate is grafted onto the hollow microspheres by using a silane coupling agent; the silane coupling agent is at least one of KH550, KH560, KH570 and Si69.
2. The method for preparing hollow microspheres modified with glycidyl methacrylate according to claim 1, characterized in that: Here are the steps: (1) adding a silane coupling agent to anhydrous ethanol to prepare an anhydrous ethanol solution of the silane coupling agent; placing the dried hollow microspheres into the anhydrous ethanol solution of the silane coupling agent, stirring at a speed of 600-700 rpm in a water bath at 60° C.-70° C. for 1 h-2 h; washing the obtained sample three times to remove the unreacted silane coupling agent, and drying for later use; (2) The sample prepared in step (1) is added to DMF, and then glycidyl methacrylate is added dropwise to the solution, and AIBN is added as an initiator, and then the mixed solution is stirred at 600-700 rpm in a water bath at 80-85° C. for 4-5 h; the obtained sample is repeatedly washed with acetone and methanol and thoroughly dried to obtain glycidyl methacrylate modified hollow microspheres.
3. The method for preparing hollow microspheres modified with glycidyl methacrylate according to claim 2, characterized in that: The silane coupling agent is at least one of KH550 and KH570.
4. Use of the glycidyl methacrylate modified hollow microspheres prepared by the method of claim 2 or 3 in the preparation of hollow microsphere / natural rubber composite materials.
5. A hollow microsphere / natural rubber composite material, characterized in that: The glycidyl methacrylate modified hollow microspheres prepared by the method of claim 2 or 3 are used as fillers.
6. The hollow microsphere / natural rubber composite material according to claim 5, characterized in that: The invention is prepared from the following components in parts by mass: 100 parts of natural rubber, 20 parts of carbon black, 30 parts of glycidyl methacrylate modified hollow microspheres prepared by the method described in claim 2 or 3, 4 parts of zinc oxide, 2 parts of stearic acid, 2.5 parts of antioxidant 4020, 5 parts of paraffin oil, 1.5 parts of sulfur, and 1.3 parts of accelerator CZ.
7. The method for preparing the hollow microsphere / natural rubber composite material according to claim 6, characterized in that: Here are the steps: (1) NR, carbon black, hollow microspheres modified with glycidyl methacrylate, zinc oxide, stearic acid, antioxidant 4020, and paraffin oil are added to an internal mixer and mixed for 5-10 minutes. After the rubber is discharged and cooled to room temperature, sulfur and accelerator CZ are added and mixed on an open mixer. After mixing evenly, the mixture is cooled down; (2) placing the rubber mixture obtained in step (1) into a flat vulcanizer for vulcanization to obtain a hollow microsphere / natural rubber composite material.
8. The method for preparing the hollow microsphere / natural rubber composite material according to claim 7, characterized in that: The temperature of the internal mixer was set at 90° C., and the rotor speed was set at 80 r / min.
9. The method for preparing the hollow microsphere / natural rubber composite material according to claim 7, characterized in that: The vulcanization is performed at a temperature of 150° C., a pressure of 10 MPa, and a time of 1.3×Tc90.