Low-gloss waterborne polyurethane resin capable of being thinly coated and preparation method thereof
By optimizing the components and processes of water-based polyurethane resin, the problems of low gloss and high hiding strength are solved, and the formation of low gloss coating film on film or paper is achieved, which improves leveling performance and adhesion and reduces costs. Meets the needs of high-end decorative materials.
Patent Information
- Application Number
- CN202411116443.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-22
AI Technical Summary
When the existing low-gloss water-based polyurethane resin is applied on a film or paper substrate, it is difficult to achieve low gloss and high hiding force, and the leveling performance and adhesion are insufficient, and the coating thickness is difficult to meet performance requirements. Reduce, affecting cost-effectiveness.
By optimizing the polymer components and process flow, a low-gloss, thin-coated aqueous polyurethane resin is prepared, including polytetramethylene ether glycol, isocyanate, carboxylic acid group-containing diol, sulfonate salt philtrum Water chain extenders, etc., control particle size and molar ratio, add thickeners and defoamers to form resins with excellent rheology properties and hiding power.
It is achieved to form a defect-free wet film of no more than 4 μm on PET, BOPP film or paper, with low gloss, excellent adhesion and thick skin feeling, reducing the cost of use, and improving the storage stability and leveling performance of the resin.
Abstract
Description
Technical Field
[0001] The invention relates to a water-based polymer resin for water-based paint or water-based ink, and in particular to a low-gloss, thinly-coated water-based polyurethane resin and a preparation method thereof. Background Art
[0002] Waterborne polyurethane resin has the characteristics of being environmentally friendly and non-toxic, having adjustable hardness and softness, good film-forming properties, good adhesion to the substrate, and good mechanical properties. It is widely used as the main resin component of waterborne coatings, inks, and adhesives.
[0003] For water-based paint, a coating film is formed on the substrate, thereby giving the substrate surface protective properties and decorative properties. The decorative effect of water-based paint is one of the key application properties of the paint. The glossiness of the coating film formed by the paint is one of the key indicators that reflect the decorative performance of the paint. With the development of the popular trend of decorative materials and the changes in consumer aesthetics, films or papers coated with matte surfaces are widely used in the outer packaging of high-end goods, such as cigarette boxes, wine boxes, mobile phone boxes, gift boxes, clothing labels, etc. Compared with materials decorated with bright surfaces, packaging materials decorated with matte surfaces have better visual effects and can better reflect a sense of high-end. At the same time, they can cover up some defects of the substrate and give the packaging materials a special feel, such as a warm touch.
[0004] During the application process, low-gloss waterborne polyurethane resin is generally used in combination with high-gloss waterborne resin, so that it is easy to obtain a coating with medium gloss (60° gloss is 10~50GU) and adjustable gloss, and the mechanical properties, adhesion and scratch resistance of the coating can be taken into account. However, to obtain low-gloss (60° gloss is 0~3GU) or even completely matte (60° gloss is 0~0.6GU) film packaging materials or cardboard, low-gloss waterborne polyurethane resin cannot be mixed with other waterborne resins, and low-gloss waterborne polyurethane resin needs to be directly applied to the film packaging material or cardboard substrate. This places higher requirements on the leveling performance, adhesion and scratch resistance of low-gloss waterborne polyurethane resin. Moreover, as market competition becomes increasingly fierce, in order to reduce costs, when applying low-gloss water-based polyurethane resins, the coating thickness of the coating will be reduced as much as possible while meeting the requirements of application performance. For example, the wet film thickness must not exceed 4μm, which further puts higher requirements on the leveling performance and hiding power of the low-gloss water-based polyurethane resin coating.
[0005] Patent CN110204740A discloses a self-matting polyurethane aqueous dispersion, which is prepared by an acetone method, and discloses that the gloss of the prepared water-based paint coating is less than 0.5GU at 60°. However, the invention does not involve the coating thickness of the coating film, the thin coating leveling performance on substrates such as films or paper, and the hiding power. Patent CN110183611A discloses a water-based polyurethane self-matting resin, which is applied to printing paste, and does not involve the coating thickness of the coating film, the thin coating leveling performance on substrates such as films or paper, and the hiding power. The coating thickness and construction method of the printing paste are completely different from those of the coating used for films or paper. Summary of the invention
[0006] In order to solve the above problems, the present invention provides a low-gloss, thin-coatable water-based polyurethane resin and a preparation method thereof. The water-based polyurethane resin obtained by the present invention has excellent rheological properties and good hiding power, and can directly form a defect-free wet film of no more than 4 μm on a film substrate such as PET, BOPP or a paper substrate, thereby saving the use cost. Moreover, the obtained coating film has low gloss, good adhesion and a thick skin feel.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows: A low-gloss, thinly-coated water-based polyurethane resin, comprising the following components in parts by mass: 70-90 parts of polytetramethylene ether glycol A, 30-50 parts of polytetramethylene ether glycol B, 55-75 parts of diisocyanate, 2.5-5 parts of diol containing carboxylic acid group, 1-4 parts of diol chain extender, 1.5-4 parts of neutralizer, 7-20 parts of amine chain extender, 1-2 parts of sulfonate hydrophilic chain extender, 300-500 parts of deionized water, 6-20 parts of thickener, 3-10 parts of leveling agent; 3-10 parts of defoamer.
[0008] Furthermore, the number average molecular weight Mn of the polytetramethylene ether glycol A is 600-1100 g / mol, and the number average molecular weight of the polytetramethylene ether glycol B is 1900-2100 g / mol.
[0009] Furthermore, the molar ratio of polytetramethylene ether glycol A to polytetramethylene ether glycol B is (3-5):1 The diol containing carboxylic acid group is one or more of dimethylol propionic acid and dimethylol butyric acid. The sulfonate hydrophilic chain extender is one or more of sodium ethylenediamine ethanesulfonate (AAS) and PPS.
[0010] In parts by mass, the mass ratio of the diol containing a carboxylic acid group to the resin solids is 1.5-2.5%.
[0011] Furthermore, the molar ratio of the diol containing a carboxylic acid group to the sulfonate hydrophilic chain extender is 10 to 1:1; more preferably 9 to 5:1.
[0012] In the preparation process of the waterborne polyurethane resin of the present invention, the amount range and molar ratio of the diol containing carboxylic acid group and the sulfonate hydrophilic chain extender are controlled to obtain a waterborne polyurethane resin with large particle size that can be redispersed.
[0013] The so-called redispersibility means that after the large-particle water-based polyurethane resin emulsion that has not been thickened with a thickener has been left to stand for more than one day, or the finished water-based polyurethane resin product obtained after thickening has been left to stand for more than three months, the polymer particles in the water-based resin will sink to the bottom to form solid agglomerates. The solid agglomerates are placed in deionized water and dispersed to form a water-based emulsion or water-based resin again. This process is called redispersibility.
[0014] The average particle size of the waterborne polyurethane obtained by the present invention is 1200-1600 nm, and the testing method is a dynamic light method using a Malvern laser particle size analyzer for testing.
[0015] If only carboxylic acid group-containing diols are selected as hydrophilic chain extenders, or the proportion of carboxylic acid group-containing diols in the hydrophilic chain extender is too high, the resulting resin will form a coagulant after precipitation and cannot be dispersed into an emulsion, resulting in poor storage stability of the resin, which in turn makes the resin unusable.
[0016] If only sulfonate hydrophilic chain extender is used as the hydrophilic chain extender, or the proportion of sulfonate hydrophilic chain extender in the hydrophilic chain extender is too high, it will be difficult to emulsify the resin when dispersing it. This is because the sulfonate hydrophilic chain extender reacts with the isocyanate group through the amino group, and its reaction is too violent, which easily forms flocs that are difficult to disperse. In addition, the particle size of the waterborne polyurethane resin is difficult to control, and thus it is difficult to control the reproducibility of the resin production.
[0017] The diisocyanate includes one or more of isophorone diisocyanate, hexamethylene diisocyanate, and 4,4-dicyclohexylmethane diisocyanate, which are diols containing carboxylic acid groups and sulfonate hydrophilic chain extenders; more preferably, it is a combination of isophorone diisocyanate and 4,4-dicyclohexylmethane diisocyanate. Further, the molar ratio of isophorone diisocyanate to 4,4-dicyclohexylmethane diisocyanate is 13-5:1; more preferably, it is 12-8:1.
[0018] The diol chain extender is one or more of 1,4-cyclohexanedimethanol, neopentyl glycol, and propylene glycol; more preferably 1,4-cyclohexanedimethanol.
[0019] The neutralizing agent is one or more of triethylamine, N-methyldiethanolamine, and dimethylethanolamine. Further, the neutralizing agent is preferably triethylamine.
[0020] The amine chain extender is one or more of ethylenediamine, isophoronediamine, hydrazine hydrate, 1,4-cyclohexanediamine, diethylenetriamine and triethylenetetramine; more preferably, it is a combination of 1,4-cyclohexanediamine or 1,4-cyclohexanediamine and any one of ethylenediamine, isophoronediamine, hydrazine hydrate and diethylenetriamine.
[0021] The present invention adds a thickener component during the preparation of the waterborne polyurethane resin, the purpose of which is to prevent the sedimentation of particles in the waterborne polyurethane resin, which leads to poor storage stability of the resin. At the same time, the thickened resin has certain rheological properties and can be directly coated on a substrate.
[0022] The thickener is preferably a combination of an acrylate thickener and a polyurethane thickener, and more preferably a combination of Dow Chemical ASE-60 and Rohm and Haas RM-2020.
[0023] The leveling agent is one or more of BYK333 or tego280; the defoamer is one or more of tego904W, BYK-011, and BYK021. The purpose of adding a small amount of defoamer to the resin in the present invention is mainly to eliminate bubbles generated when the resin is thickened, so as to avoid the difficulty in eliminating bubbles in the resin after the viscosity of the resin increases after thickening. Adding a small amount of leveling agent can eliminate the negative impact of leveling caused by adding defoamer to the resin.
[0024] The dosage of the thickener, leveling agent and defoamer can be adjusted by technicians through experiments according to the application indexes of the resin.
[0025] The low-gloss, thinly-coated water-based polyurethane resin provided by the present invention has a solid content of 28-36%, and more preferably 30-34%.
[0026] The coating-4 cup viscosity (test temperature is 25° C.) of the low-gloss, thinly-coated water-based polyurethane resin provided by the present invention is 40 to 80 seconds, and more preferably 45 to 60 seconds.
[0027] The present invention provides a water-based polyurethane self-matting resin that can be thinly coated, and a preparation method thereof comprises the following steps: Step S1, adding measured amounts of polytetramethylene ether glycol A, B, diol containing carboxylic acid group, and diol chain extender into a reaction kettle, heating, stirring, vacuumizing, heating and dehydrating at 120° C. for 20-40 min, then cooling to 60° C. and passing nitrogen; Step S2, adding a measured amount of diisocyanate, heating to 85°C for reaction for 2-4h, and then cooling to 50°C; Step S3, adding a measured neutralizing agent and neutralizing for 30 to 60 minutes, and continuing to cool to room temperature; Step S4, adding a measured amount of sulfonate sulfonate hydrophilic chain extender and reacting for 10 to 20 minutes, and then adding a measured amount of deionized water and dispersing at high speed for 30 to 60 minutes; Step S5, adding a measured amount of amine chain extender and continuing high-speed dispersion for 20 to 40 minutes; Step S6, adding a measured amount of thickener, leveling agent, and defoamer in any order and continuing high-speed dispersion for 20 to 40 minutes, stopping the dispersion, and obtaining a dispersion liquid; Step S7, filtering the dispersion with a 400-mesh filter cloth, adding a proper amount of deionized water to adjust the solid content, and obtaining a finished product of a water-based polyurethane self-matting resin that can be thinly coated.
[0028] The invention also provides an application of a low-gloss, thinly-coated water-based polyurethane resin, which can be used for surface coating of films, paper and clothing.
[0029] The beneficial effects of the present invention are as follows: The invention prepares a waterborne polyurethane resin with low gloss and thin coating, good rheological properties and excellent hiding power by optimizing the components and dosage of polymer diol, isocyanate, diol chain extender and diamine chain extender in the raw materials. The obtained resin has low gloss, can achieve a full matte effect, has good storage stability, and has a thick hand feel and a strong skin feel. DETAILED DESCRIPTION
[0030] The present invention will be further described below in conjunction with specific embodiments: It should be understood that the specific embodiments described herein are part of the embodiments of the present invention, rather than all of the embodiments, and are merely used to explain the embodiments of the present invention, and are not used to limit the embodiments of the present invention. All other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0031] For the purpose of simplicity and illustration, the principles of the embodiments are described mainly by reference to examples. In the following description, many specific details are proposed to provide a thorough understanding of the embodiments. However, it is obvious. For those of ordinary skill in the art, these embodiments may not be limited to these specific details in practice. In some instances, known methods and structures are not described in detail to avoid making these embodiments unnecessarily difficult to understand. In addition, all embodiments may be used in combination with each other.
[0032] The raw materials for preparing low-gloss, thin-coatable waterborne polyurethane resins are as follows: Polytetramethylene ether glycol A, Mn is about 1000 g / mol, purchased from BASF; polytetramethylene ether glycol B, Mn is about 2000 g / mol, purchased from BASF; isophorone diisocyanate, hexamethylene diisocyanate, 4,4-dicyclohexylmethane diisocyanate were all purchased from Wanhua Chemical; sodium ethylenediamine sulfonate (AAS) was purchased from Evonik; dimethylol propionic acid was purchased from Perstorp.
[0033] Unless otherwise specified, other raw materials were commercially available. Example 1
[0034] Step S1, by weight, 80 parts of polytetramethylene ether glycol A (Mn is about 1000 g / mol), 40 parts of polytetramethylene ether glycol B (Mn is about 2000 g / mol), 4 parts of dimethylol propionic acid, and 3.5 parts of 1,4-cyclohexanedimethanol are added to a reaction kettle, the temperature is increased, stirring is started, vacuum is drawn, heating and dehydration is performed at 120° C. for 20 minutes, and then the temperature is reduced to 60° C. and nitrogen is passed through; Step S2, add 65 parts of isophorone diisocyanate, raise the temperature to 85°C for reaction for 4 hours, and then cool down to 50°C; Step S3, adding 3 parts of triethylamine to neutralize for 30 minutes, and continuing to cool to room temperature; Step S4, adding 1.5 parts of sodium ethylenediamine sulfonate (AAS) hydrophilic chain extender and reacting for 15 minutes, then adding 455 parts of deionized water and dispersing at high speed for 30 minutes; Step S5, adding 17 parts of 1,4-cyclohexanediamine and continuing high-speed dispersion for 20 minutes; Step S6, adding 6.7 parts of ASE-60 thickener, 5.5 parts of RM-2020 thickener, 3 parts of tego280 leveling agent, and 2 parts of tego904W defoamer in any order, and continuing to disperse at high speed for 20 minutes, stopping the dispersion, and obtaining a dispersion liquid; Step S7, filtering the dispersion with a 400-mesh filter cloth, adding deionized water to adjust the solid content to about 32%, thereby obtaining a low-gloss, thinly-coated water-based polyurethane resin product. Example 2
[0035] Compared with Example 1, the difference is that the isophorone diisocyanate in Example 1 is replaced by an equimolar amount of 4,4-dicyclohexylmethane diisocyanate. Example 3
[0036] Compared with Example 1, the difference is that the isophorone diisocyanate in Example 1 is replaced by an equimolar amount of hexamethylene diisocyanate. Example 4
[0037] Compared with Example 1, the difference is that the isophorone diisocyanate in Example 1 is replaced by a combination of isophorone diisocyanate and 4,4-dicyclohexylmethane diisocyanate in equimolar amounts. The molar ratio of isophorone diisocyanate to 4,4-dicyclohexylmethane diisocyanate is 10:1. Example 5
[0038] Compared with Example 1, the difference is that the isophorone diisocyanate in Example 1 is replaced by a combination of isophorone diisocyanate and 4,4-dicyclohexylmethane diisocyanate in equimolar amounts. The molar ratio of isophorone diisocyanate to 4,4-dicyclohexylmethane diisocyanate is 3:1. Example 6
[0039] Compared with Example 1, the difference is that the isophorone diisocyanate in Example 1 is replaced by a combination of isophorone diisocyanate and hexamethylene diisocyanate in equimolar amounts. The molar ratio of isophorone diisocyanate to hexamethylene diisocyanate is 10:1. Example 7
[0040] Compared with Example 4, 1,4-cyclohexanedimethanol in Example 4 was replaced by an equal molar amount of 1,4-butanediol. Example 8
[0041] Compared with Example 4, the 1,4-cyclohexanediamine in Example 4 was replaced by an equal molar amount of hydrazine hydrate. Example 9
[0042] The ASE-60 thickener in Example 4 was replaced with the same amount of Dow Chemical TT-935 polyacrylate thickener. Example 10
[0043] The RM-2020 thickener in Example 4 was replaced with the same amount of Lamberti VISCOLAM PS166 polyurethane thickener.
[0044] Comparative Example 1 When the total molar amount of hydroxyl groups remains unchanged, the molar ratio of polytetramethylene ether glycol A to polytetramethylene ether glycol B is adjusted to 2:1.
[0045] Comparative Example 2 When the total molar amount of hydroxyl groups remains unchanged, the molar ratio of polytetramethylene ether glycol A to polytetramethylene ether glycol B is adjusted to 6:1.
[0046] Physical index test of the resin obtained in Examples 1-10 and Comparative Examples 1-2 Solid content: Weigh 1-2g of resin and place it on aluminum foil. Bake at 120℃ until constant weight is reached. Test the dry weight and calculate the solid content. Keep 2 significant figures for the result.
[0047] Viscosity: At 25°C, use a Tu-4 cup to test the viscosity of the resin.
[0048] Application index test of the resin obtained in Examples 1-10 Storage stability test: Take 200g of resin and put it into a plastic bottle, put it into a 60℃ oven, and record the stability of the resin every 2 days until the resin delaminates or gels. The longest test time is 30 days.
[0049] Gloss test: The resin was coated on the Biugeda hiding test card (surface coated card) with an OSP-4 wire rod, with a wet film thickness of 4μm. After baking at 60℃ for 1min until the coating was dry, the 60° gloss of the black base was tested with a gloss meter.
[0050] Hiding power test: The resin is coated on the Biugeda hiding power test cardboard (surface coated cardboard) with an OSP-4 wire rod, with a wet film thickness of 4μm. The hiding power effect is visually inspected based on the exposed bottom, with scores ranging from 1 to 5 from poor to good.
[0051] Leveling test: The resin is coated on the Biugeda hiding test cardboard (surface coated cardboard) with an OSP-4 wire rod, and the wet film thickness is 4μm. The leveling performance of the wet film is visually inspected based on the shrinkage, leveling, and drawing degree of the wet film, with scores ranging from 1 to 5 from poor to good.
[0052] Feel: The resin was coated on the Biugeda hiding power test cardboard (surface coated cardboard) with an OSP-4 wire rod, with a wet film thickness of 4μm. After baking at 60℃ for 1min until the coating was dry, the coating was touched back and forth with the thumb, and the comprehensive skin feel and thickness were scored, with scores from 1 to 5 from bad to good.
[0053] Table 1 Physical indexes and application performance test table of waterborne polyurethane resin Test items Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Example 8 Example 9 Example 10 Comparative Example 1 Comparative Example 2 Solid content (%) 32.1 32.3 32.1 32.3 32.0 32.2 32.0 32.2 32.1 31.9 32.2 32.1 Viscosity (seconds) 55.6 72.8 88.3 58.2 62.1 65.6 54.3 48.8 28.6 86.3 57.4 76.6 Storage stability 30 days OK 6 days demulsification 10 days demulsification 30 days OK 24 days demulsification 26 days of emulsion breaking 30 days OK 30 days OK 2 days stratification 30 days OK 30 days OK 4 days demulsification 60° Gloss (GU) 0.4 0.3 2.6 0.4 0.3 0.8 0.4 0.5 0.6 0.7 1.2 0.4 Covering power 4 5 5 5 5 4 3 2 4 3 1 2 Leveling 5 5 5 5 5 5 4 3 5 4 1 2 Feel 3 1 1 5 3 1 2 2 4 4 3 1 From the test results of Example 1 and Examples 4-8 in Table 1, it can be seen that the waterborne polyurethane resin obtained by using isophorone diisocyanate as the diisocyanate, more preferably a diisocyanate composed of isophorone diisocyanate and 4,4-dicyclohexylmethane diisocyanate in a molar ratio range of 13 to 5:1, and using 1,4-cyclohexanedimethanol as the diol chain extender and 1,4-cyclohexanediamine as the diamine chain extender has low gloss, excellent thermal storage stability, hiding power and leveling properties, and good feel.
[0054] In Example 2, 4,4-dicyclohexylmethane diisocyanate was used as the diisocyanate raw material, and the hardness of the obtained resin was too high, and the hand feel of the resin was poor. In addition, the emulsification effect of the resin was poor, and the storage stability was deteriorated.
[0055] In Example 3, hexamethylene diisocyanate is used as the diisocyanate raw material. Since hexamethylene diisocyanate is a soft linear structure, it is difficult to obtain large-size particles, and the glossiness of the obtained resin becomes larger, and a low-gloss coating film cannot be obtained. In addition, the compatibility of the resin and the thickener is poor, the viscosity of the thickened resin is high, and the phenomenon of continuous thickening will occur during storage, resulting in poor stability of the resin.
[0056] The hydrophobically modified alkali swelling thickener TT-935 used in Example 9 replaces ASE-60. The low shear viscosity of the obtained resin becomes smaller, the resin forms stratification during storage, and the storage stability of the resin is poor.
[0057] The hydrophobically modified polyurethane thickener PS-166 used in Example 10 was used to replace the RM-2020 thickener. The low shear viscosity of the obtained resin increased, resulting in poor hiding power and leveling properties of the resin.
[0058] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A low-gloss, thinly-coated water-based polyurethane resin, characterized in that: The raw materials for preparing the waterborne polyurethane resin include the following components in parts by mass: 70-90 parts of polytetramethylene ether glycol A, 30-50 parts of polytetramethylene ether glycol B, 55-75 parts of diisocyanate, 2.5-5 parts of diol containing carboxylic acid group, 1-4 parts of diol chain extender, 1.5-4 parts of neutralizer, 7-20 parts of amine chain extender, 1-2 parts of sulfonate hydrophilic chain extender, 300-500 parts of deionized water, 6-20 parts of thickener, 3-10 parts of leveling agent; 3-10 parts of defoamer; The number average molecular weight Mn of the polytetramethylene ether glycol A is 900-1100 g / mol, and the number average molecular weight Mn of the polytetramethylene ether glycol B is 1900-2100 g / mol.
2. The aqueous polyurethane resin according to claim 1, characterized in that: Calculated on a solid basis, the molar ratio of the diol containing a carboxylic acid group to the sulfonate hydrophilic chain extender is 10 to 1:
1.
3. The aqueous polyurethane resin according to claim 1, characterized in that: The diol containing a carboxylic acid group is one or more of dimethylol propionic acid and dimethylol butyric acid.
4. The aqueous polyurethane resin according to claim 1, characterized in that: The diisocyanate includes one or more of isophorone diisocyanate, hexamethylene diisocyanate, and 4,4-dicyclohexylmethane diisocyanate; preferably, it is a combination of isophorone diisocyanate and 4,4-dicyclohexylmethane diisocyanate.
5. The waterborne polyurethane resin according to claim 1, characterized in that: The diol chain extender is one or more of 1,4-cyclohexanedimethanol, neopentyl glycol, and propylene glycol; more preferably 1,4-cyclohexanedimethanol; the neutralizer is one or more of triethylamine, N-methyldiethanolamine, and dimethylethanolamine.
6. The aqueous polyurethane resin according to claim 1, characterized in that: The amine chain extender is one or more of ethylenediamine, isophoronediamine, hydrazine hydrate, 1,4-cyclohexanediamine, diethylenetriamine and triethylenetetramine; preferably 1,4-cyclohexanediamine.
7. The waterborne polyurethane resin according to claim 1, characterized in that: The sulfonate hydrophilic chain extender is one or more of sodium ethylenediamine ethanesulfonate and PPS.
8. The waterborne polyurethane resin according to claim 1, characterized in that: The thickener is a combination of an acrylic thickener and a polyurethane thickener, preferably a combination of ASE-60 and Rohm and Haas RM-2020; the leveling agent is one or more of BYK333 or tego280; the defoaming agent is one or more of tego904W, BYK-011, and BYK021.
9. The method for preparing an aqueous polyurethane resin according to any one of claims 1 to 8, characterized in that: The steps include: Step S1, adding measured amounts of polytetramethylene ether glycol A, B, diol containing carboxylic acid group, and diol chain extender into a reaction kettle, heating, stirring, vacuumizing, heating and dehydrating at 120° C. for 20-40 min, then cooling to 60° C. and passing nitrogen; Step S2, adding a measured amount of diisocyanate, heating to 85°C for reaction for 2-4h, and then cooling to 50°C; Step S3, adding a neutralizing agent for neutralization for 30 to 60 minutes, and continuing to cool to room temperature; Step S4, adding a sulfonate sulfonate hydrophilic chain extender and reacting for 10 to 20 minutes, and then adding deionized water for high-speed dispersion for 30 to 60 minutes; Step S5, adding an amine chain extender and continuing high-speed dispersion for 20 to 40 minutes; Step S6, adding a thickener, a leveling agent, and a defoamer in any order and continuing to disperse at high speed for 20 to 40 minutes, stopping the dispersion, and obtaining a dispersion liquid; Step S7, filtering the dispersion with a 400-mesh filter cloth, adding a proper amount of deionized water to adjust the solid content, and obtaining a finished product of a water-based polyurethane self-matting resin that can be thinly coated.
10. The use of the waterborne polyurethane resin according to any one of claims 1 to 8, characterized in that: Used for direct coating on the surface of BOPP film, PET film, and decorative cardboard substrates; or as a gloss adjustment resin for water-based coatings and water-based inks.