High-wear-resistance polyurethane mechanical part material and preparation method thereof
By introducing nano-alumina particles and molybdenum disulfide into polyurethane materials and using precise preparation and surface treatment technology, the problem of insufficient wear resistance of polyurethane materials in high wear environments is solved, and the material performance is significantly improved and application scope is achieved. extension.
Patent Information
- Application Number
- CN202411114862.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-22
AI Technical Summary
The existing polyurethane materials lack wear resistance and durability in high load and high speed wear environments, resulting in increased maintenance costs and reduced reliability of mechanical components.
Nanoalumina particles and molybdenum disulfide are used as reinforcement materials and wear-resistant modifiers, combined with precise preparation methods and surface treatment technology, a high-wear-resistant polyurethane material is developed to improve its wear resistance and mechanical strength.
It significantly improves the wear resistance and mechanical strength of the material, extends the service life of the components, reduces the frequency of maintenance and replacement, meets the application needs in high wear environments, and improves the chemical stability and production efficiency of the material.
Smart Images

Figure CN118994534A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, in particular to the synthesis and application of polyurethane materials with high wear resistance. Background Art
[0002] Polyurethane materials are widely used in the industrial field to manufacture various mechanical parts, including but not limited to bearings, gears and sliders, due to their excellent physical properties and chemical stability. These parts are subjected to continuous friction and wear during mechanical operation, which places extremely high demands on the wear resistance of the materials. Although polyurethane materials perform well in many aspects, their wear resistance still needs to be improved in high-load and high-speed wear environments.
[0003] Most polyurethane materials on the market are general or standard types. They perform well in conventional applications, but under extreme conditions, such as high loads, high-speed rotation or chemical corrosion environments, the wear resistance and durability of these materials often cannot meet industrial needs. This leads to increased maintenance costs and faster replacement frequency of mechanical parts, which in turn affects the stability and reliability of the entire mechanical system.
[0004] In order to improve the wear resistance of polyurethane materials, researchers have tried a variety of methods, including using different chemical formulas, adding various fillers and reinforcing materials. However, these methods often only provide limited performance improvements, or sacrifice other properties of the material, such as elasticity and toughness, while improving wear resistance. Therefore, the development of a new polyurethane material that can significantly improve wear resistance while maintaining other excellent properties of polyurethane materials is of great significance to promoting industrial development and reducing production costs.
[0005] Based on such background and needs, the present invention has developed a new type of highly wear-resistant polyurethane material by in-depth research on the chemical structure and physical properties of polyurethane materials, innovatively introducing specific nanoparticle reinforcement materials and wear-resistant modifiers. This material not only achieves a significant improvement in wear resistance, but also further expands its application range in high-wear environments while maintaining the original advantages of polyurethane materials.
[0006] Technical solution:
[0007] The purpose of the present invention is to provide a highly wear-resistant polyurethane material and a preparation method thereof to meet the stringent requirements of mechanical parts under high wear environments on material properties. The material has excellent wear resistance, mechanical strength and stability, and is suitable for manufacturing key mechanical parts such as bearings, gears, and sliders.
[0008] High wear-resistant polyurethane material is an innovative polymer composite material whose composition is carefully designed to achieve excellent wear resistance and mechanical strength. The following is a detailed description of each component:
[0009] Polyether or polyester polyol: As one of the basic components of polyurethane materials, the polyol selected in the present invention accounts for 55-65% of the total weight. These polyols have a number average molecular weight between 2000-8000, ensuring the flexibility and elasticity of the material. The hydroxyl value is in the range of 200-400 mg KOH / g. This specific hydroxyl value range helps control the reaction rate and the crosslinking density of the final product, thereby obtaining ideal mechanical properties.
[0010] Isocyanate: Isocyanate is a key raw material for forming polyurethane. The present invention uses 4,4'-diphenylmethane diisocyanate (MDI), accounting for 35-45% of the total weight. MDI is selected because it has high reactivity and excellent chemical stability. MDI with a purity of at least 99.5% ensures the uniformity of the reaction and the consistency of the performance of the final product.
[0011] Nanoparticle reinforcement material: The nano-alumina introduced in the present invention as a reinforcement material accounts for 5-8% of the total weight. The average particle size of the nano-alumina is controlled at 20-50 nanometers, and this particle size range helps to achieve uniform dispersion and reinforcement of the material. The addition of nanoparticles significantly improves the hardness and wear resistance of the material while maintaining appropriate toughness.
[0012] Wear-resistant modifier: In order to further improve the wear resistance of the material, the present invention selects molybdenum disulfide as a wear-resistant modifier, accounting for 1-4% of the total weight. Molybdenum disulfide is evenly dispersed in the polyurethane matrix in the form of micron-sized powder, and its layered structure forms a lubricating film on the surface of the material, effectively reducing the friction coefficient and reducing wear.
[0013] Catalyst and stabilizer: The use of catalyst and stabilizer is crucial in the synthesis process of polyurethane. The present invention selects organic tin compounds as catalysts, and the amount is precisely controlled to be 0.01-0.1% of the total reactant mass. This dosage range ensures the efficient reaction and avoids the brittleness of the material caused by excessive cross-linking. The use of stabilizers helps to prevent thermal or oxidative degradation of the material during processing and use, ensuring the long-term stability of the material.
[0014] Through the precise design and optimization of the above material composition, the high wear-resistant polyurethane material of the present invention achieves a significant improvement in wear resistance while maintaining the original excellent performance of polyurethane, meeting the application requirements of mechanical parts in high wear environments.
[0015] 2. Preparation method: The preparation method of the highly wear-resistant polyurethane material of the present invention comprises the following steps:
[0016] Step a) Prepolymerization: In this step, firstly, accurately measured polyether or polyester polyol is mixed with 4,4'-diphenylmethane diisocyanate (MDI) under nitrogen protection. The reaction temperature is strictly controlled at 60-80°C to avoid the occurrence of side reactions. This temperature range is conducive to controlling the reaction rate and ensuring the uniform molecular structure of the prepolymer. The time of the prepolymerization reaction is adjusted according to the progress of the reaction until the desired prepolymer viscosity is reached.
[0017] Step b) Dispersion of reinforcing materials and modifiers: After the prepolymer is formed, slowly add the pre-weighed nano-alumina particles and molybdenum disulfide powder. Use a high shear mixer to stir at a high speed of 3000-5000 rpm to ensure that the nano-particles and modifiers are evenly dispersed in the prepolymer. This process is crucial because uniform dispersion directly affects the final properties of the material, especially wear resistance and mechanical strength.
[0018] Step c) Addition of catalyst and stabilizer: Add catalyst and stabilizer to the uniformly mixed mixture. The catalyst is added to accelerate the subsequent curing reaction, while the stabilizer is used to improve the thermal stability and aging resistance of the material during processing and use. The mixing process continues until all components are completely uniformly dispersed without visible phase separation.
[0019] Step d) Casting: The uniformly mixed material is poured into a pre-prepared mold under precisely controlled conditions. The design and surface treatment of the mold have an important influence on the shape and surface quality of the final product. After pouring, the material is cured at room temperature for 24 hours. This step allows the material to initially form a stable three-dimensional network structure.
[0020] Step e) Post-curing: The pre-cured parts are post-cured at 110-130°C for 2-4 hours. This step is key to ensuring that the material is fully cross-linked and achieves maximum hardness and strength. Precisely controlled post-curing conditions can optimize the final properties of the material.
[0021] Step f) Vacuum post-curing: Finally, the parts are post-cured in a vacuum environment. This step helps remove tiny bubbles inside the material and further improves the density and uniformity of the material. Vacuum treatment can also reduce oxidation and other side reactions that may affect material performance.
[0022] Through precise control and optimization of each step of the above-mentioned preparation method, the highly wear-resistant polyurethane material of the present invention exhibits excellent performance, including significantly improved wear resistance, enhanced mechanical strength and excellent chemical stability, meeting the stringent requirements for mechanical component materials in high wear environments.
[0023] In the preparation process of the highly wear-resistant polyurethane material of the present invention: after the initial curing and post-curing treatment, the parts are thoroughly cleaned and surface pretreated to ensure the firm adhesion of the coating or plating. This step includes removing oil, rust and oxides on the surface, laying a solid foundation for subsequent surface treatment. One or more layers of wear-resistant and corrosion-resistant coatings are applied to the surface of the parts using advanced coating technology. The selection of coatings depends on the application environment and performance requirements of the parts, and may include polytetrafluoroethylene, ceramic particles or specific polymers. The coating process is carried out by precisely controlled spraying, dipping or brushing technology to ensure that the coating is evenly covered to form a smooth and uniform protective film. According to the special needs of the parts, plating technology may be used to further enhance its surface properties. A layer of metal or non-metallic film, such as nickel, chromium, gold, silver or tungsten carbide, is deposited on the surface of the parts by methods such as electroplating, chemical plating, physical vapor deposition (PVD) or chemical vapor deposition (CVD). This film not only improves the hardness and wear resistance of the parts, but also may give them conductivity, reflectivity or other special functions. In order to further improve the wear resistance and service life of the components, surface hardening treatment becomes a key step. Using laser, electron beam or induction heating technology, the surface of the component is quickly heated and cooled to form a hardened layer with higher hardness and wear resistance. This hardened layer exhibits excellent performance when subjected to high loads and wear. After the coating or plating is completed, the component will undergo a fine polishing treatment to obtain a smoother surface and higher gloss. This step is carried out by hand or mechanical polishing equipment to ensure that the appearance and feel of the component meet industrial standards. Each surface-treated component will undergo a series of rigorous quality inspections, including surface roughness testing, hardness testing, adhesion testing and corrosion resistance testing. These tests ensure that the performance of the component meets or even exceeds the design requirements and ensures reliability under extreme working conditions. Through this series of coherent surface treatment steps, the high wear-resistant polyurethane material of the present invention not only has excellent performance in the material itself, but also the surface of its molded parts is fully strengthened and protected, making it an ideal choice for extreme environments and high-load applications.
[0024] The performance test described: Wear resistance test is carried out, which is the core of evaluating material performance. The test simulates actual use conditions by placing the material sample in a specific wear test equipment, such as a rotating disc wear tester, in contact with the abrasive at a specific speed and pressure. By measuring the wear depth or mass loss of the material over a certain period of time, its wear resistance is quantitatively analyzed. The test results are presented in the form of wear rate, which is crucial for comparing the wear resistance of different materials. Mechanical strength test evaluates the mechanical properties of the material. This includes the determination of tensile strength, compressive strength and impact strength. The sample is subjected to tensile and compression tests using a universal material testing machine to determine its maximum load-bearing capacity and elastic modulus. Impact strength testing is completed through Charpy impact testing, which evaluates the toughness of the material when subjected to rapid impact. These test results comprehensively reflect the performance of the material when subjected to dynamic and static loads. Stability testing is key to ensuring the long-term performance of the material. Thermal stability testing is carried out by placing the sample in a high temperature environment for a certain period of time and then measuring the changes in its physical properties. Chemical resistance testing evaluates its corrosion resistance by immersing the sample in different chemical media, such as acid, alkali or salt solutions. Weathering tests simulate natural conditions such as UV exposure, humidity and temperature changes to evaluate material aging and performance degradation. For parts that have been treated with coatings or plating, an evaluation of the surface treatment effect is essential. This includes testing the adhesion, hardness and corrosion resistance of the coating. Adhesion tests are performed by cross-cut or tape methods to determine the bonding strength of the coating to the substrate. Hardness tests use a durometer to measure the surface hardness of the coating, while corrosion resistance tests are completed through chemical immersion tests. Comprehensive performance evaluation combines all the above test results to evaluate the performance of the material in actual applications. This may include long-term operation tests that simulate actual working conditions to observe the performance changes of the material under continuous load and wear conditions. Through these tests, we can ensure the reliability and durability of the material in high-wear environments, providing users with confidence.
[0025] Through the above technical scheme, the present invention successfully solves the problem of insufficient performance of existing polyurethane materials in high-wear environments, and provides a new material option with better performance and greater durability for the industrial field.
[0026] The above technical solution can bring the following three key technical effects:
[0027] 1. Excellent wear resistance improvement: The reason why the highly wear-resistant polyurethane material of the present invention has excellent wear resistance is that nano-alumina particles are carefully introduced into the chemical formula. Such particles are evenly dispersed in the polyurethane matrix with a precise weight percentage of 5-8% and an average particle size controlled within the range of 20-50 nanometers. The high hardness and excellent dispersibility of nano-alumina provide the material with a wear-resistant layer at a microscopic level, which not only significantly improves the surface hardness of the material, but also forms a solid protective barrier on the surface of the material, effectively resisting sliding friction and wear. In practical applications, especially in parts that are subject to high wear such as bearings and gears, the improvement in the wear resistance of this material directly translates into a longer service life, reducing the frequency of maintenance and replacement, thereby significantly reducing long-term operating costs.
[0028] 2. Optimized balance between mechanical strength and toughness: The addition of molybdenum disulfide wear-resistant modifier is the key to achieving a balance between mechanical strength and toughness in the present invention. This modifier is evenly dispersed in the material at a precise ratio of 1-4%. Its micron-sized powder form not only significantly improves the self-lubrication of the material and reduces the friction coefficient, but also provides additional toughness when the material is subjected to stress due to its layered structure. When the material is subjected to impact or bending, the layered structure of molybdenum disulfide can absorb and disperse energy, thereby preventing the expansion of cracks and enhancing the material's resistance to fracture. This balanced mechanical property is achieved by precisely controlling the amount of modifier added and the dispersion process, ensuring that the material maintains high strength while also having excellent toughness, making it more suitable for withstanding complex and variable mechanical loads.
[0029] 3. Efficient production and processing adaptability: The preparation method of the present invention ensures the uniformity and processing adaptability of the material through high shear mixing and post-curing treatment steps. During the high shear mixing process, the nanoparticles and modifiers are evenly dispersed under high-speed stirring at 3000-5000 rpm. This process effectively avoids agglomeration and ensures the uniformity of the microstructure of the material, thereby improving the overall performance of the material. The post-curing treatment is carried out at a temperature of 110-130°C for 2-4 hours. This step enhances the cross-linking density of the material, improves the stability of the material and the dimensional accuracy of the molded parts. The post-curing treatment under a vacuum environment further reduces the bubbles in the material and improves the density of the material. These optimized preparation processes not only improve the performance of the material, but also make the material easy to mass produce, meeting the dual requirements of production efficiency and cost-effectiveness in industrial applications. Through these processes, the production efficiency of the material is improved while maintaining the consistency and reliability of the material, providing an efficient and economical solution for industrial applications.
[0030] These three technical effects not only reflect the breakthrough of the present invention in material performance, but also demonstrate its practical value and potential economic impact in actual industrial applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is the prepolymerization reaction flow chart of the present invention
[0032] Figure 2 This is the surface treatment flow chart of the present invention
[0033] Figure 3 The preparation diagram of the highly wear-resistant polyurethane material of the present invention DETAILED DESCRIPTION
[0034] The following will be combined with the attached embodiment of the present invention Figure 1 , the technical solutions in the embodiments of the present invention are clearly and completely described. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] In the preparation process of the highly wear-resistant polyurethane material of the present invention, a detailed description of the specific implementation is as follows, including the detailed operation and parameter setting of each step:
[0036] In a nitrogen-protected environment, first accurately weigh the polyether or polyester polyol and 4,4'-diphenylmethane diisocyanate (MDI). Mix the polyol and MDI at a precise molar ratio, and strictly control the reaction temperature at 60-80°C. This temperature range is selected to ensure the uniformity of the reaction rate and avoid side reactions caused by too fast a reaction. The time of the prepolymerization reaction is adjusted according to the progress of the reaction, usually 1-3 hours, until the desired prepolymer viscosity is reached, and the viscosity range is controlled at 500-1500cP. During this process, the pressure and stirring rate inside the reactor are also continuously monitored to ensure the consistency of the reaction conditions and the uniformity of the reaction.
[0037] After the prepolymer is formed, the pre-weighed nano-alumina particles and molybdenum disulfide powder are slowly added. Use a high shear mixer at a high speed of 3000-5000 rpm for 15-30 minutes to ensure that the nanoparticles and modifiers are evenly dispersed in the prepolymer. This process is critical because uniform dispersion directly affects the final properties of the material, especially wear resistance and mechanical strength. During this step, the power consumption of the mixer and the temperature change of the material are also monitored to ensure the consistency of the dispersion effect.
[0038] Add catalyst and stabilizer to the homogenized mixture. The catalyst is usually an organotin compound, and the amount is 0.05-0.08% of the total reactant mass. The choice of stabilizer depends on the final application environment of the material, and may include antioxidants, UV absorbers, etc., and the amount is controlled at 0.1-0.3%. The mixing process continues until all components are completely evenly dispersed without visible phase separation. During this step, the pH value and conductivity of the mixture are also monitored to ensure the uniform distribution of the catalyst and stabilizer.
[0039] The uniformly mixed material is poured into a pre-prepared mold under precisely controlled conditions. The mold design should take into account the shape and size of the final product, and the surface should be polished to reduce the generation of bubbles. After pouring, the material is cured at room temperature for 24 hours. This step allows the material to initially form a stable three-dimensional network structure. During this process, the temperature and humidity of the mold will also be controlled to ensure the consistency of the curing process.
[0040] The pre-cured parts are post-cured at 110-130°C for 2-4 hours. This step is key to ensuring that the material is fully cross-linked and reaches maximum hardness and strength. Precisely controlled post-curing conditions can optimize the final properties of the material. During this step, the thermal expansion coefficient and thermal conductivity of the parts are also monitored to ensure the effectiveness of the post-curing treatment.
[0041] Finally, the parts are post-cured in a vacuum environment. The vacuum level is controlled at 0.1-1.0 mbar and the post-curing time is extended to 4-6 hours. This step helps to remove tiny bubbles inside the material, further improving the density and uniformity of the material. The vacuum treatment can also reduce oxidation and other side reactions that may affect the performance of the material. During this step, the air pressure and temperature in the vacuum chamber are also monitored to ensure the effectiveness of the vacuum post-curing treatment.
[0042] After the initial curing and post-curing treatment, the parts are thoroughly cleaned and surface pre-treated to ensure the strong adhesion of the coating or plating. This step includes removing oil, rust and oxide on the surface to lay a solid foundation for subsequent surface treatment. The cleaning process may include solvent cleaning, ultrasonic cleaning or sandblasting.
[0043] Advanced coating technology is used to apply one or more layers of wear-resistant and corrosion-resistant coatings to the surface of the component. The choice of coating depends on the application environment and performance requirements of the component, and may include polytetrafluoroethylene, ceramic particles or specific polymers. The coating process is carried out through precisely controlled spraying, dipping or brushing techniques to ensure uniform coverage of the coating to form a smooth, uniform protective film. The thickness and uniformity of the coating are key parameters and are usually monitored by coating thickness gauges.
[0044] Depending on the special needs of the component, coating technology may be used to further enhance its surface properties. A layer of metal or non-metallic film, such as nickel, chromium, gold, silver or tungsten carbide, is deposited on the surface of the component by methods such as electroplating, chemical plating, physical vapor deposition (PVD) or chemical vapor deposition (CVD). This film not only improves the hardness and wear resistance of the component, but may also give it conductivity, reflectivity or other special functions. The thickness and uniformity of the coating are key parameters and are usually monitored by surface analysis techniques such as X-ray diffraction or scanning electron microscopy.
[0045] In order to further improve the wear resistance and service life of the components, surface hardening becomes a key step. Using laser, electron beam or induction heating technology, the surface of the component is quickly heated and cooled to form a hardened layer with higher hardness and wear resistance. This hardened layer exhibits excellent performance when subjected to high loads and wear. The effect of surface hardening is usually evaluated through hardness testing and wear testing.
[0046] After coating or plating, the parts will undergo a fine polishing process to obtain a smoother surface and higher gloss. This step is performed by hand or mechanical polishing equipment to ensure that the appearance and feel of the parts meet industrial-grade standards. The polishing process may include wet polishing, dry polishing or mechanical polishing, and the surface roughness after polishing is usually monitored by a surface roughness tester.
[0047] After the prepolymerization reaction is completed, the viscosity of the prepolymer is first accurately measured to ensure that it is in the range of 500-1500cP using a rotational viscometer at 25°C. At the same time, the chemical structure is verified using a Fourier transform infrared spectrometer (FTIR) to ensure that no side reactions occur in the prepolymer and the purity of the molecular design is maintained.
[0048] After the reinforcement and modifier dispersion step, the dispersion of the reinforcement and modifier in the prepolymer is observed by optical microscopy or scanning electron microscopy (SEM) to ensure that the particles are evenly distributed and free of agglomeration. In addition, the uniform distribution of the catalyst and stabilizer is checked by wet chemical analysis methods, such as inductively coupled plasma mass spectrometry (ICP-MS), to ensure that their concentrations are in the range of 0.05-0.08% and 0.1-0.3%, respectively.
[0049] The curing degree after casting is measured by differential scanning calorimetry (DSC) to evaluate the crosslinking degree and glass transition temperature (Tg) of the material. After the post-curing treatment is completed, the Shore hardness of the material is measured using a durometer to ensure that it is within the range of 90-100A, and the tensile strength and elongation at break are measured using a universal material testing machine.
[0050] After vacuum post-curing treatment, X-ray computed tomography (CT) is used to detect the density and bubble content inside the material. The goal is to control the bubble content below 0.5% to ensure the uniformity and density of the material.
[0051] After coating or plating is completed, the coating thickness is measured using a coating thickness gauge to ensure that it is within the range of 50-200 microns. Adhesion testing is performed using the cross-cut method or tape method to ensure that the coating adhesion grade is not less than 5B. Corrosion resistance testing is performed in a salt spray test chamber to ensure that the coating corrosion resistance time in 3.5% NaCl solution is not less than 500 hours.
[0052] The hardness of the surface hardened layer is measured using a microhardness tester to ensure that it is at least 30% harder than the base material. The wear resistance is measured using a wear tester to ensure that the wear resistance of the hardened layer is improved by at least 50%.
[0053] After polishing, the surface roughness is measured using a surface roughness tester to ensure that the Ra value is within the range of 0.1-0.4 microns. The surface gloss is measured using a gloss meter to ensure that it reaches a reflectivity of more than 90%.
[0054] Each component will be inspected for dimensional accuracy and shape accuracy using a three-dimensional coordinate measuring machine or laser scanner to ensure that the dimensional tolerance of the component is controlled within ±0.05 mm.
[0055] Through this series of meticulous and comprehensive quality inspection steps, the high wear-resistant polyurethane material of the present invention is strictly monitored in each production link, ensuring the consistency and reliability of the material and meeting the stringent requirements for mechanical component materials in a high wear environment.
[0056] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only preferred examples of the present invention and are not intended to limit the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A highly wear-resistant polyurethane material, characterized in that: The invention is composed of the following components in weight percentage: 55-65% of polyether or polyester polyol, 35-45% of isocyanate, 5-8% of nano-particle reinforcing material, 1-4% of wear-resistant modifier, and proper amount of catalyst and stabilizer.
2. The highly wear-resistant polyurethane material according to claim 1, characterized in that: The polyether or polyester polyol has a number average molecular weight between 2000 and 8000, and a hydroxyl value between 200 and 400 mg KOH / g.
3. The highly wear-resistant polyurethane material according to claim 1, characterized in that: The isocyanate is 4,4'-diphenylmethane diisocyanate (MDI) with a purity of at least 99.5%.
4. The highly wear-resistant polyurethane material according to any one of claims 1 to 3, characterized in that: The nano-particle reinforcement material is nano-aluminum oxide, the average particle size of which is 20-50 nanometers and the content of which is 6-7%.
5. The highly wear-resistant polyurethane material according to any one of claims 1 to 4, characterized in that: The wear-resistant modifier is molybdenum disulfide, the content of which is 1.5-3.5%, and is evenly dispersed in the polyurethane matrix in the form of micron-sized powder.
6. A method for preparing the highly wear-resistant polyurethane material according to any one of claims 1 to 5, characterized in that The following steps are involved: a) Under nitrogen protection, polyol and isocyanate are subjected to prepolymerization reaction at 60-80° C. to form a prepolymer; b) nanoparticle reinforcement material and wear-resistant modifier are added to the prepolymer, and a high shear mixer is used to disperse the prepolymer at a stirring speed of 3000-5000 rpm until a uniform mixture is formed; c) a catalyst and a stabilizer are added, and mixing is continued until the mixture is completely uniform; d) the mixture is cast in a mold, and then cured at room temperature for 24 hours; e) a post-curing treatment is performed at a temperature of 110-130° C. for 2-4 hours to obtain a highly wear-resistant polyurethane material.
7. The preparation method according to claim 6, characterized in that: The catalyst for the prepolymerization reaction is an organic tin compound, and the amount used is 0.01-0.1% of the total amount of reactants.
8. The preparation method according to claim 6 or 7, characterized in that: The high shear mixer used in the reinforcing material dispersing step has at least two stirring blades with different diameters to achieve uniform dispersion in three-dimensional space.
9. The preparation method according to any one of claims 6 to 8, characterized in that: The post-curing treatment is performed in a vacuum environment to reduce bubbles in the material and improve the density of the material.
10. A highly wear-resistant polyurethane mechanical component, characterized in that: The component is made of the highly wear-resistant polyurethane material described in any one of claims 1 to 5, and the component is subjected to special surface treatment, such as coating or plating, to further improve its wear resistance and corrosion resistance.
Citation Information
Cited By
Preparation process optimization method and system based on high-heat-resistance wire enamel