Method for detinning and purifying PLGA (poly (lactic-co-glycolic acid)) crude product prepared by ring-opening polymerization method

Through the ring-opening polymerization method and glacial acetic acid solvent system, the tin ions in PLGA were successfully removed and polymer degradation was inhibited, which solved the problems of tin ion removal and polymer stability in the prior art, and achieved efficient PLGA purification and pharmaceutical use Improve the quality of auxiliary materials.

CN118994551APending Publication Date: 2024-11-22ZHEJIANG SUNDOC PHARMA SCI & TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411113021.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing PLGA purification technology cannot effectively remove tin ions and reduce polymer degradation, resulting in unstable quality of pharmaceutical excipients and difficult to meet the limit requirements of the pharmacopoeia for tin content.

Method used

The crude PLGA product was prepared by ring-opening polymerization method, dissolved and precipitated with a mixed solvent containing glacial acetic acid, and obtained refined PLGA by vacuum drying, achieving effective removal of tin ions and improving the stability of the polymer.

Benefits of technology

The tin ion residue is less than 30ppm, the polymer molecular weight remains above 95%, and the molecular weight distribution index remains unchanged, which avoids polymer degradation and meets the quality requirements of pharmaceutical excipients.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004992830760000041
    Figure BDA0004992830760000041
  • Figure BDA0004992830760000081
    Figure BDA0004992830760000081
  • Figure BDA0004992830760000111
    Figure BDA0004992830760000111
Patent Text Reader

Abstract

The invention discloses a detinning purification method of a PLGA (poly (lactic-co-glycolic acid)) crude product prepared by a ring-opening polymerization method, which comprises the following steps: (1) dissolving the PLGA crude product prepared by the ring-opening polymerization method in a mixed solvent containing glacial acetic acid at room temperature to obtain a PLGA crude product solution; and (2) dropwise adding the PLGA crude product solution into a precipitant according to a volume ratio of the PLGA crude product solution to the precipitant of 1: (6-11), filtering, collecting a precipitate, and carrying out vacuum drying and crushing on the precipitate to obtain refined PLGA. The detinning agent has a good detinning effect and can effectively inhibit polymer degradation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of pharmaceutical excipient purification, and in particular to a tin removal and purification method for a PLGA crude product prepared by a ring-opening polymerization method. Background Art

[0002] Poly(Lactide-Co-Glycol) (hereinafter referred to as PLGA) is an environmentally friendly, biodegradable, non-toxic material. It has been approved as a pharmaceutical excipient in different countries. PLGA plays the role of a drug carrier in some complex injection categories, such as microsphere preparations and implants, and mainly controls drug release through its own degradation behavior, so that the preparation can achieve the purpose of long-term sustained release.

[0003] There are two main ways to synthesize PLGA, one is direct polycondensation and the other is ring-opening polymerization. Direct polycondensation is time-consuming, inefficient, and cannot obtain high molecular weight (unless otherwise specified, "molecular weight" refers to weight average molecular weight) PLGA. Ring-opening polymerization can control the synthesis of low or high molecular weight PLGA in a short time under the action of a catalyst. It has a wider range of applications and is widely used in industrial production. The catalyst commonly used in the ring-opening polymerization industry is a tin-containing compound, which is classic, efficient, and cheap.

[0004] When PLGA is used in drug preparations, it is necessary to remove small molecular weight oligomers and unreacted polymerized monomers in the crude product that may affect the sudden release of the drug, reduce the content of tin ions introduced by the catalyst, and meet the quality requirements for pharmaceutical excipients.

[0005] Commonly used methods include solvent precipitation, supercritical fluid extraction, and dialysis. Although supercritical fluid extraction conforms to the advantages of green chemistry and no organic solvent use, it cannot achieve industrial purification of PLGA due to its high technical difficulty, complex pipeline design, high-pressure equipment, and lack of mature equipment and technology in China. The dialysis method achieves the purpose of removing small molecular weight oligomers and monomers by controlling the molecular weight cutoff of the membrane, but it cannot reduce the content of tin ions in the bonded catalyst, and is not suitable for industrial large-scale purification. The conventional solvent precipitation method is to dissolve PLGA in a good solvent, and then drip in a precipitant that is several times the good solvent. The precipitant is used to dissolve monomers and small molecular weight oligomers. During the dripping process, PLGA is precipitated in the precipitant, and the finished product is obtained by filtration and drying. Although this method can remove monomers and oligomers, the use of its precipitant is also prone to polymer degradation and molecular weight reduction, and it still cannot reduce the content of catalyst tin ions.

[0006] In order to overcome the above shortcomings and obtain a low-tin content, stable polymer that meets the quality standard requirements of pharmaceutical excipients, the prior art also uses extraction to reduce the tin content.

[0007] For example, in the process of refining glycolide-lactide copolymer, a method for removing organic tin was proposed (Yang Li, Luan Hansen, Xu Fenglan, et al. [J]. Chinese Journal of Pharmaceutical Industry, 2013, 44 (3): 3). An extraction method was proposed to effectively remove stannous octoate from PLGA. PLGA was dissolved in acetonitrile, and an equal volume of petroleum ether was added to prepare a solution with a concentration of 1%. After 30 minutes, the solution was allowed to stand for stratification. The acetonitrile layer was separated and extracted with the same volume of petroleum ether for 3 times, and the solvent was evaporated to obtain refined PLGA. Although the petroleum ether extraction method has a good tin removal effect, the operation is complicated and requires multiple extractions. The concentration of the PLGA solution required is extremely low, which makes the amount of organic solvent used for industrial production too large, the drying cycle is long and inefficient, and the equipment requirements are high, which is prone to danger. In addition, other purification methods need to be combined to remove oligomers and monomers, which reduces the feasibility of practical application.

[0008] Another example is CN101466758A which discloses a biodegradable and bioabsorbable polymer with a low metal catalyst content and a preparation method thereof. In the presence of a metal catalyst, lactide (lactic acid cyclic dimer) and ε-caprolactone are copolymerized in a predetermined molar ratio, washed with a mixed solvent containing acetic acid and isopropanol in a volume ratio of 25 / 75 to 45 / 55 at a temperature below 40°C, and the copolymer is dried. The mixed solvent is exchanged more than 5 times, and the washing time is more than 48 hours in total. The washed copolymer is dried at 20°C to 35°C for 10 to 30 hours, and then dried at 35°C to 50°C for 40 to 100 hours. The content of the metal catalyst can be reduced to less than 1ppm in terms of metal. The mixed solvent has the function of wetting the polymer so that acetic acid and the metal catalyst form a chelate and the chelate is extracted into the solution. However, the specification mentioned that the polymer was dissolved because it contained a large amount of acetic acid. The method used a large amount of acetic acid for pickling, and the mixed solvent washing time was long. It also required multiple exchanges for washing with low efficiency and complicated process. The optimal molecular weight retention rate after drying was more than 80%, indicating that the polymer dissolved in a large amount of acetic acid had been significantly degraded and the molecular weight was significantly reduced; under its drying conditions, the polymer obtained had a high acetic acid residue, which affected the storage stability of the polymer and its use in preparations.

[0009] JP2021193160A discloses a method for producing a purified polyester copolymer with a small amount of residual tin catalyst. The solution of the tin-containing polyester copolymer is adjusted to a concentration of 5-20wt%, and the solvent added to the solution containing the tin-containing polyester copolymer includes, for example, chloroform, dimethyl ether, dichloromethane, acetone, N,N-dimethylformamide, ethyl acetate, tetrahydrofuran, acetonitrile, xylene, water, etc. Acid is then added to the concentrated solution to react with the tin catalyst, preferably acetic acid and / or hydrochloric acid is added as acid, and the amount of acid added is 0.5-20 parts by weight per 100 parts by weight of the tin-containing polyester copolymer. The temperature is 20°C-50°C to promote the efficiency of the acid reaction. After the acid reaction, a washing step of washing with water is performed to reduce the acid remaining in the tin-containing polyester copolymer. To fully remove the acid, it is preferably washed more than 3 times. There is also a reprecipitation step after the acid reaction step, and the liquid polyester copolymer is added dropwise to the reprecipitation solvent, and the reprecipitation solvent includes methanol, ethanol, isopropanol, hexane, etc. Finally, the precipitate is dried under reduced pressure to obtain a purified polyester copolymer from which the tin catalyst has been removed. The technical effect of the purification method of the invention is that the refined polyester copolymer preferably has a residual tin content of less than 300ppm, which cannot meet the requirements of the Chinese Pharmacopoeia (2020 edition) (hereinafter referred to as the Pharmacopoeia) for the PLGA tin content limit of less than 150ppm. And it cannot guarantee the consistency of the molecular weight of the polyester copolymer before and after the purification process, and the process requires long-term heating for the acid reaction step and the water washing step to remove the acid residue, and then through the reprecipitation step, it is prepared by reduced pressure drying. Each step is prone to cause significant degradation of the polymer, and the molecular weight of the polymer decreases more significantly with the extension of the treatment time. This method avoids the technical problem of molecular weight reduction during the purification process, and does not disclose the acid residue of the polyester copolymer after purification. Tin removal also brings about the influence of other unstable factors, which is not suitable for the application of pharmaceutical-grade polyester copolymers.

[0010] CN101939355A also discloses a method for purifying a polymer and a method for producing a polymer using the same, which are used to inhibit the molecular weight reduction of the polymer and effectively reduce the residual catalyst in the polymer. It preferably uses an organic solvent containing lactic acid as a catalyst removal solvent, and contacts the polymer with the catalyst removal solvent for 1 to 24 hours at a temperature of 30 to 55°C. The concentration of the organic acid in the catalyst removal solvent is 0.5 to 4 mol / L, and the ratio (v / w) of the catalyst removal solvent to the polymer is 2 or more. It also includes a monomer removal process for removing monomer residues, and a method for further contacting the polymer with a solvent containing an organic solvent, which is different from the aforementioned catalyst removal solvent and preferably does not contain the aforementioned organic acid, inorganic acid and other acids. After the aforementioned catalyst removal process and before the aforementioned monomer removal process, there may also be a process for removing organic acids. The removal of organic acids from the polymer, for example, the polymer after the aforementioned catalyst removal process is contacted with a solvent, and the treatment time is not particularly limited, for example, 0.5 to 2 hours, preferably 1 hour. This method is prone to polymer degradation starting from the time when the polymer is impregnated with an organic solvent preferably containing lactic acid. The polymer molecular weight data after 24 hours of immersion in the embodiment has been significantly reduced, and the use of multiple organic solvents in the subsequent organic acid removal process and monomer removal process is not conducive to the subsequent solvent removal process and drying process.

[0011] Existing PLGA purification technology, while removing metal ions, polymer monomers, oligomer impurities and organic solvents, cannot effectively inhibit polymer degradation, resulting in a significant decrease in polymer molecular weight, making it difficult to ensure the consistency of the molecular weight of the polymer before and after the purification process, and even avoiding the technical problem of significant degradation of the polymer after purification. Generally speaking, the smaller the molecular weight of PLGA, the faster the degradation and the shorter the drug release cycle, so the significant reduction in polymer molecular weight can easily lead to abnormal drug release behavior. Therefore, as a polymer for pharmaceutical excipients, considering the quality stability of the excipients and the requirements for formulation stability, the purification process should be able to effectively inhibit polymer degradation, so that the weight average molecular weight of the polymer after purification is consistent, should not be less than 95.0% of the original weight average molecular weight before purification, and the molecular weight distribution index (hereinafter referred to as PDI) should not be significantly increased. Therefore, it is necessary to develop a simple and efficient purification method to obtain PLGA that meets the needs of pharmaceutical excipients. Summary of the invention

[0012] The object of the present invention is to provide a method for removing tin and purifying a crude PLGA product prepared by a ring-opening polymerization method, which has a good tin removal effect and can effectively inhibit polymer degradation.

[0013] The technical solution adopted by the present invention to solve its technical problem is: A method for removing tin and purifying a crude PLGA product prepared by a ring-opening polymerization method comprises the following steps: (1) dissolving a crude PLGA product prepared by a ring-opening polymerization method in a mixed solvent containing glacial acetic acid at room temperature to obtain a crude PLGA solution; (2) Slowly adding the crude PLGA solution to the precipitant, the volume ratio of the crude PLGA solution to the precipitant being 1:6-11, collecting the precipitate by filtration, vacuum drying and crushing the precipitate to obtain refined PLGA.

[0014] The present invention adopts a mixed solvent consisting of a PLGA organic good solvent and glacial acetic acid to dissolve a PLGA crude product, and then obtains a PLGA finished product through solvent precipitation and vacuum drying. The glacial acetic acid in the mixed solvent can prompt PLGA to complete a chain termination elementary reaction, improve the stability of PLGA during the purification process, and can be effectively removed in the subsequent purification process.

[0015] Glacial acetic acid is widely used in pharmaceutical preparations. In the present invention, a small amount of glacial acetic acid is introduced and effectively removed, and there is no need to re-evaluate the impact of a small amount of acetic acid residue in the purified polymer on the pharmaceutical preparation. The purification method disclosed in the present invention is simple to operate, has good safety, and is suitable for industrial production. The good solvent and precipitant used are common solvents for commercial PLGA, which are recorded and limited in pharmacopoeias, and can be directly used as pharmaceutical excipients.

[0016] Because the catalyst tin ions are chemically bonded to the polymer ends (as shown below), neither dialysis nor conventional solvent precipitation methods can break the chemical bonds and reduce the residual tin ions. Because the crude PLGA obtained from industrial high-temperature production is in a dense glass state after cooling, oxygen and moisture in the air cannot penetrate, so the chain termination elementary reaction is not completely carried out. This is the reason why conventional purification methods cannot reduce the tin ion content. High tin content not only affects the use of the preparation due to biological toxicity, but also the tin ion end-capping will activate the group, the polymer chain is easy to break, and it is easy to cause the polymer weight-average molecular weight to decrease and the PDI to become wider;

[0017] The ring-opening polymerization method is to copolymerize lactide and glycolide as raw materials under the action of a metal tin catalyst in an inert environment to obtain a crude PLGA product. The crude PLGA product can be prepared according to the prior art or commercially available. The preparation method of the ring-opening polymerization of the crude PLGA is not particularly limited. The weight average molecular weight of the crude PLGA of the method of the present invention is preferably 2 to 10w.

[0018] The research team of the present invention found that the prior art often first dissolves the PLGA crude product in an organic good solvent to form a crude solution of a certain concentration. Since PLGA, as a high molecular polymer, has a certain viscosity when it is dissolved to form a solution, the addition of glacial acetic acid is not conducive to the uniform distribution of glacial acetic acid in the crude solution. In order to fully chelate and remove the tin ions at the ends of PLGA in the crude solution, it is often necessary to increase the amount of glacial acetic acid used. However, the increase in the amount of glacial acetic acid used can easily cause the degradation of the polymer and also bring a burden to the subsequent acid removal step. Therefore, while the prior art ensures the tin removal effect, it can easily cause obvious degradation of the polymer and it is difficult to maintain the molecular weight of the original polymer, thereby causing changes in the physical and chemical properties related to the molecular weight of the polymer.

[0019] The research team of the present invention has made a breakthrough by first uniformly mixing glacial acetic acid with a low volume ratio with an organic good solvent to form a mixed solvent. At this time, the glacial acetic acid in the mixed solvent is evenly distributed and has an extremely low concentration, which is less likely to cause the possibility of accelerated degradation of PLGA when it contacts a high concentration acid environment. At the same time, it is more conducive to the full combination of glacial acetic acid with the tin ions of the PLGA crude product. As the mixed solvent dissolves the PLGA crude product, the glacial acetic acid evenly distributed in the mixed solvent can continuously and stably chelate the catalyst tin ions that are difficult to remove at the end of the polymer, making them free in the PLGA crude product solution.

[0020] At the same time, the research team of the present invention also unexpectedly discovered that the specific volume ratio of glacial acetic acid combined with the purification method of the subsequent steps of the present invention has an inflection point tin removal effect. When the amount of glacial acetic acid is too much or too little, the tin removal effect is weakened or significantly weakened; and the inflection point tin removal effect is significant, and the consistency of the tin removal effect can be ideally achieved. After purification of different batches of crude polymer products, the tin residue can be stably controlled to be below 50ppm, and more ideally controlled to be below 30ppm, which is far lower than the requirement of 150ppm or less in the pharmacopoeia.

[0021] Since the present invention realizes the purification and application of glacial acetic acid with a low volume ratio, the polymer chain termination reaction is promoted to be completed, the polymer end is replaced with a hydroxyl group, the quality stability of the polymer is improved, the polymer degradation is prevented, and the disadvantages of obvious polymer degradation and PDI widening caused by tin removal in the prior art are effectively eliminated.

[0022] The concentration of the PLGA crude solution is 0.06-0.1g / mL. The solution in this concentration range has good stability and low viscosity, which is conducive to slow addition and dispersion in the subsequent precipitation step, and is fully dissolved and precipitated in the low-temperature precipitant environment of the present invention. The PLGA crude product is dissolved in a mixed solvent to form a low-concentration PLGA crude solution, and the volume change before and after dissolution is negligible, so the volume of the mixed solvent can be regarded as the volume of the PLGA crude solution. Further, in order to reduce the amount of precipitant and mixed solvent used, the preferred PLGA crude solution concentration is 0.08-0.1g / mL. In order to promote dissolution, an auxiliary stirring method can also be included. The ideal stirring method is to fully mix and promote dissolution without the action of strong shear force. For example, a paddle downward pressure stirring is used, and the stirring speed is 200-250rpm to dissolve for 2 to 4 hours to form a transparent clear solution, and the PLGA crude solution is obtained for complete dissolution. The present invention does not limit the mixed dissolution method.

[0023] The mixed solvent containing glacial acetic acid is composed of glacial acetic acid and a good solvent for PLGA, wherein the volume ratio of glacial acetic acid is 5-20%. Preferably, in order to reduce the residual amount of glacial acetic acid and take into account the tin removal effect, the volume ratio of glacial acetic acid in the mixed solvent containing glacial acetic acid is 8-10%. The glacial acetic acid described in the present invention is commercially available anhydrous glacial acetic acid, preferably chromatographically pure glacial acetic acid.

[0024] The good solvent for PLGA is one of dichloromethane and acetone or a combination of the two.

[0025] Preferably, the volume ratio of the PLGA crude solution to the precipitant is 1:7-10, more preferably 1:7-8. The volume ratio of the low-concentration PLGA crude solution to the low-temperature precipitant of the present invention is used to ensure that the PLGA crude solution is dispersed in the low-temperature precipitant to fully dissolve and precipitate, and has a good removal effect on monomers, oligomer impurities, tin ions and glacial acetic acid. If the volume of the precipitant is too small, the purification effect is poor, which is not conducive to sufficient dissolution to remove monomers, oligomer impurities, tin ions and glacial acetic acid. If the volume of the precipitant is too large, the amount of organic solvent is large, and the purification effect does not change significantly. The PLGA crude solution is slowly added to the low-temperature precipitant, and sufficient contact promotes rapid dissolution and precipitation. The method of slow addition is not particularly limited, such as adding in the form of small droplets by dripping, or adding in the form of low-speed spraying, or adding in the form of a low-speed small liquid flow, etc.

[0026] The precipitant is one of methanol and ethanol or a combination of the two. The precipitant has an ideal dissolving effect on monomers and oligomers, but does not dissolve PLGA. The precipitant also needs to be miscible with the mixed solvent.

[0027] The temperature of the precipitant is controlled below -2°C. Preferably, the temperature of the precipitant is controlled at -10°C to -2°C. The low temperature environment of the precipitant is conducive to inhibiting the hydrolysis of the ester bond of the PLGA polymer, and promoting the rapid precipitation of the PLGA polymer in the precipitant to form precipitated particles, which is convenient for dispersion and collection. If the temperature of the precipitant is extremely low, the energy consumption is large, and the solubility of the crude polymer monomer or oligomeric impurities in the precipitant is reduced, resulting in a relatively higher monomer residue in the finished product. However, at an extremely low temperature of -20°C, the monomer residue of the finished product can still achieve the purpose of being lower than the pharmacopoeia requirements. Compared with the finished product obtained at -2 to -10°C, the monomer residue is relatively high, so -2 to -10°C is more preferred. When the temperature of the precipitant is high, the precipitated PLGA particles are severely adhered, the sample is uneven, and the purification effect is not ideal.

[0028] Vacuum drying includes the initial drying stage and the main drying stage: Initial drying stage: temperature 30-40°C, vacuum degree -101kPa, drying for 3-4h; Main drying stage: heat to 50-60°C, vacuum degree to -101kPa, dry for 24h.

[0029] The research team of the present invention has found that the precipitated particles obtained in the above steps are very likely to cause polymer degradation if they are immediately subjected to high-temperature vacuum drying. Through exploratory research, it was found that the initial drying stage under specific conditions can unexpectedly achieve the ideal purpose of quickly removing most of the residual solvent, and then enter the main drying stage to remove the remaining small amount of solvent. Through the pioneering specific segmented vacuum drying of the present invention, polymer degradation can be effectively inhibited, and solvent residues and glacial acetic acid residues can be reduced.

[0030] The finished product obtained after vacuum drying is taken out and crushed to a particle size of 5 to 10 mm to obtain a purified finished product. The most ideal aspect of the present invention is to obtain a purified finished product with consistent molecular weight before and after purification, narrow distribution, less than 30 ppm tin residue, no glacial acetic acid residue, and stable quality.

[0031] The beneficial effects of the present invention are: The present invention fully mixes an organic good solvent for PLGA with glacial acetic acid with a low volume percentage, and then uses the mixed solvent to dissolve a crude PLGA product, so that the glacial acetic acid and the tin ions of the crude PLGA product are fully chelated, the polymer chain termination unit reaction is promoted to be complete, and the quality stability of the polymer is improved. The glacial acetic acid with a low volume percentage of the present invention is significantly superior to the use of other organic acids.

[0032] The low-concentration PLGA crude product solution of the present invention is precipitated by a low-temperature precipitant, and the precipitate is vacuum-dried, so as to achieve the purpose of simultaneously removing impurities including glacial acetic acid, tin ions, monomers and oligomers, and the ideal control of glacial acetic acid residue can be achieved without an additional acid removal process, and the most ideal is to achieve no glacial acetic acid residue. At the same time, the low-temperature environment of the precipitation step can effectively inhibit the degradation of the polymer and promote the precipitation of PLGA, and the specific segmented vacuum drying step of the present invention can also effectively inhibit the degradation of the polymer and effectively shorten the drying time.

[0033] The purification process of glacial acetic acid with a specific volume ratio of the present invention has a tin removal effect with an inflection point, and the tin removal effect with the inflection point is significant. The tin residue in different batches of crude PLGA can be stably controlled to be below 50 ppm, and more ideally to be controlled to be below 30 ppm, which is much lower than the requirement of 150 ppm or less for PLGA excipients in the pharmacopoeia, does not cause the risk of excessive tin ions, and has a simple process, is suitable for industrial batches, and has a high purification yield.

[0034] The purification method of the present invention can effectively inhibit the degradation of the polymer, ideally maintain the physical and chemical properties related to the original polymer molecular weight, and significantly improve the quality requirements such as the stability of the polymer and its preparation after purification on the basis of the original polymer molecular weight, thereby avoiding the influence of the polymer on the pharmaceutical preparation due to the significant reduction in molecular weight after purification, and achieving the purpose of maintaining the consistency of the polymer molecular weight before and after purification while fully ensuring the tin removal effect, that is, achieving the weight average molecular weight of the finished PLGA as a pharmaceutical excipient is not less than 95.0% of the weight average molecular weight of the original crude product, and the PDI should not be significantly increased. It is more ideal to achieve the weight average molecular weight of the finished PLGA after purification of the present invention is not less than 98.0% of the weight average molecular weight of the original crude product, and under ideal control, the PDI has a tendency to decrease.

[0035] The present invention can purify the crude PLGA product without a high-temperature environment, effectively avoiding the safety risk of purification preparation at a high temperature in the presence of multiple solvents, improving the safety of the purification process, having no special equipment requirements, high purification yield, and being universal for different types of PLGA.

[0036] The purification scale can be expanded to 1-30 kg according to the needs of pharmaceutical preparations, but those skilled in the art can easily think of changes in batch scale after considering the instructions and the disclosure, and these changes still fall within the scope of protection of the present invention. The present invention has universal applicability and is applicable to PLGA with a weight average molecular weight of 2w-10w, a molar ratio of lactide of 50-95%, and a molar ratio of glycolide of 5-50%.

[0037] According to the purification method of the present invention, by selecting crude PLGA with the required weight-average molecular weight, a finished PLGA with the required target molecular weight after purification can be obtained with accurate control, and the yield is high, which is suitable for actual industrial application; while the purification process of crude PLGA in the prior art leads to a significant reduction in the molecular weight of the finished polymer, especially when the purified batches are different or the types of the purified crude PLGA are different, which may lead to different degrees of PLGA degradation, making it difficult to obtain a finished PLGA with the required target molecular weight, which can easily cause a huge waste of raw materials in the purification process. DETAILED DESCRIPTION

[0038] The technical solution of the present invention is further described in detail below through specific embodiments.

[0039] In the present invention, unless otherwise specified, the raw materials and equipment used can be purchased from the market or are commonly used in the art. The methods in the following embodiments, unless otherwise specified, are all conventional methods in the art.

[0040] The preparation of the crude PLGA prepared by the ring-opening polymerization method can refer to the method described in CN 110283305 A, or other commercially available crude PLGA products can be purchased. The lactide in the examples all adopts DL-lactide (manufacturer: Corbion).

[0041] Example 1 The raw materials were added according to the molar ratio of 50% lactide and 50% glycolide, the molar ratio of glycolic acid added as an initiator to the molar ratio of glycolide was 1:130, the amount of stannous isooctanoate catalyst added was 1.00‰ of the total mass of lactide and glycolide, and the crude PLGA was obtained by ring-opening polymerization at 180°C for 8h under an inert environment.

[0042] Prepare a mixed solvent of 2 L with a volume ratio of glacial acetic acid: dichloromethane = 2:8. Weigh 200 g crude PLGA (Mw = 52125, PDI = 1.71) and add it to 2 L of the mixed solvent. Stir at 250 rpm for 2.5 h until it is completely dissolved.

[0043] Use a peristaltic pump to drop into 16L of cold methanol at -6°C for precipitation. Filter and collect the precipitate, the total time is about 5.5h. Then vacuum dry. The vacuum degree is -101kPa, the initial drying temperature of vacuum drying is 30°C, the time is 3h, the main drying temperature is 55°C, the time is 24h, and a desiccant is used in the drying device to control the moisture. After drying, take out and crush into 5-10mm particles to obtain 178.5g of refined PLGA.

[0044] Tetrahydrofuran was used as solvent, and the weight average molecular weight was 51514 and the molecular weight distribution index (PDI) was 1.65 by gel permeation chromatography (hereinafter referred to as GPC). The tin content before and after purification was reduced from 301.3ppm to 24.7ppm by inductively coupled plasma atomic emission spectroscopy (hereinafter referred to as ICP), which was in line with the pharmacopoeia standard of less than 150ppm. The lactide content was reduced from 1.80% to 0.18% by high performance liquid chromatography, and the glycolide content was reduced from 0.15% to undetectable, which was in line with the pharmacopoeia standard of lactide content less than 1.5% and glycolide content less than 0.5%. The glacial acetic acid content was 0.3% by high performance liquid chromatography.

[0045] Table 1 changes the amount of precipitant and temperature, and the remaining steps and conditions are the same as in Example 1. The results are shown in the following table: Note: The formula for calculating the ratio of finished product to crude product Mw is: finished product weight average molecular weight ÷ crude product weight average molecular weight × 100% Mw is the abbreviation of weight average molecular weight The other experimental conditions were the same. Different amounts of precipitants had almost no effect on the molecular weight, but mainly affected the residual amount of the monomer. According to Table 1, the ratio of PLGA crude solution to methanol (v / v) was 1:6-11 and the temperature was below -2°C, which met the requirements. Considering the reduction of the amount of organic solvent and energy consumption as much as possible, combined with the molecular weight and PDI of the purified polymer, it is preferred to use 7 to 10 times the volume of the mixed solvent, more preferably 7 to 8 times. The preferred temperature is -10 to -2°C.

[0046] Samples 2-4 are samples obtained with the most preferred precipitant dosage and temperature conditions, with good purification effect, low monomer residue, easy collection and easy amplification, and the molecular weight remains consistent before and after purification. Sample 2 obtained 180.1g of refined PLGA, sample 3 obtained 178.5g of refined PLGA, and sample 4 obtained 181.7g of refined PLGA, with yields all greater than 88%.

[0047] Sample 5 is not within the scope of the present invention, the amount of precipitant used is too small, so the residual monomer content is high. The amount of solvent used is small, and the precipitated PLGA particles cannot be completely dispersed into the solution. In the later stage of purification, some crude PLGA is still in the mixed solvent and has not been precipitated into the precipitant. Therefore, the sample is uneven, the collection is easy to be blocked, and the purification is not ideal.

[0048] Sample 6 uses a larger amount of precipitant, and its purification effect is ideal, but it increases the burden of subsequent solvent removal, and the solvent and production costs increase.

[0049] Sample 7 was implemented at an extremely low temperature of -20°C. The precipitated PLGA particles were in good condition and easy to collect. The molecular weight of the polymer was consistent before and after purification. The lactide residue in the finished product was relatively high, but still lower than the pharmacopoeia standard, that is, the lactide content was less than 1.5%, and the purification effect was ideal. Considering that the refrigerant needs to be controlled at about -30°C, the precipitant temperature can reach -20°C, and the energy consumption is high, scaling up to production batches will increase the cost exponentially.

[0050] Sample 8 is not within the scope of the present invention. The temperature of the precipitant is high, and the precipitated PLGA particles are severely adhered. Stirring will be strongly hindered by the adhesion of the materials, and continuous external force intervention is required to maintain normal stirring. The sample adheres to the wall during the purification process, resulting in a low yield. The conditions for scaling up the batch are not met, the sample is uneven, and the glacial acetic acid residue is high. The actual output of Sample 8 is 119.6g, and the yield is 59.8%; the glacial acetic acid content is 1.14% and 1.67% respectively in two tests. The glacial acetic acid content is high and the sample is uneven. In addition, due to the high temperature of the precipitant and the lack of inhibition by the low temperature environment, the polymer undergoes a certain degree of degradation during the purification process, and the molecular weight decreases, so the purification is not ideal.

[0051] Sample 9 is not within the scope of the present invention. The amount of solvent used is too large, the temperature of the precipitant is high, the precipitated particles stick together, the sample is uneven and difficult to collect, the loss is large, the yield is low, and the feasibility of scaling up the batch is low. The sample is uneven, the glacial acetic acid residue is high, the actual yield of sample 9 is 134.4g, and the yield is 67.2%; the glacial acetic acid content is tested twice at 0.97% and 1.58%, the glacial acetic acid content is high and the sample is uneven. In addition, due to the high temperature of the precipitant and the lack of inhibition of the low temperature environment, the polymer undergoes a small degree of degradation during the purification process, and the molecular weight decreases, so the purification is not ideal.

[0052] Example 2 The raw materials were added according to the molar ratio of lactide to glycolide being 85% and 15%, the molar ratio of glycolic acid added as an initiator to the molar ratio of glycolide was 1:64, the amount of stannous isooctanoate catalyst added was 0.70‰ of the total mass of lactide and glycolide, and the crude PLGA was obtained by ring-opening polymerization at 180°C for 8h under an inert environment.

[0053] Prepare a mixed solvent of 3L with a volume ratio of glacial acetic acid: dichloromethane = 8:92. Weigh 200g crude PLGA (Mw = 95432, PDI = 1.81) and add it to 3L mixed solvent. Stir at 250rpm for 2h and completely dissolve. Use a peristaltic pump to drop into 30L, -10℃ cold methanol for precipitation. Filter and collect the precipitate for about 6.0h. Then vacuum dry. The vacuum degree is -101kPa, the initial drying temperature of vacuum drying is 35℃, the time is 3h, the main drying temperature is 55℃, the time is 24h, and a desiccant is used in the drying device to control the moisture. After drying, take out and crush into 5-10mm particles to obtain refined PLGA.

[0054] Using tetrahydrofuran as solvent, GPC was used to measure a weight average molecular weight of 96250, a molecular weight distribution index (PDI) of 1.74, which was 100.9% of the original weight average molecular weight, and the molecular weight remained consistent before and after purification. Using ICP, the tin content before and after purification was reduced from 200.3ppm to 30.1ppm, which met the pharmacopoeia standard of less than 150ppm. Using high performance liquid chromatography, the lactide content was reduced from 1.44% to 0.35%, and the glycolide content was reduced from 0.12% to undetected, which met the pharmacopoeia standard of lactide content less than 1.5%, and glycolide content less than 0.5%. Glacial acetic acid was not detected using high performance liquid chromatography. 182.3g of refined PLGA was obtained with a yield of 91.2%.

[0055] Example 3 The raw materials were added according to the molar ratio of lactide to glycolide being 95% and 5%, the molar ratio of glycolic acid added as an initiator to the molar ratio of glycolide was 1:6, the amount of stannous isooctanoate catalyst added was 1.80‰ of the total mass of lactide and glycolide, and the crude PLGA was obtained by ring-opening polymerization at 180°C for 5h under an inert environment.

[0056] Prepare a mixed solvent of 2L with a volume ratio of glacial acetic acid: dichloromethane = 1:9. Weigh 200g crude PLGA (Mw = 24480, PDI = 1.60) and add it to 2L mixed solvent. Stir at 250rpm for 2.5h and completely dissolve. Use a peristaltic pump to drop into 20L, -2℃ cold methanol for precipitation. Filter and collect the precipitate for about 5.5h. Then vacuum dry. The vacuum degree is -101kPa, the initial drying temperature of vacuum drying is 40℃, the time is 3h, the main drying temperature is 50℃, the time is 24h, and a desiccant is used in the drying device to control the moisture. After drying, take out and crush into 5-10mm particles to obtain refined PLGA.

[0057] Using tetrahydrofuran as solvent, GPC was used to measure a weight average molecular weight of 24620, a molecular weight distribution index (PDI) of 1.51, which was 100.6% of the original weight average molecular weight, and the molecular weight remained consistent before and after purification. Using ICP, the tin content before and after purification was reduced from 514.2ppm to 25.4ppm, which met the pharmacopoeia standard of less than 150ppm. Using high performance liquid chromatography, the lactide content was reduced from 2.40% to 0.17%, and the glycolide content was reduced from 0.01% to undetected, which met the pharmacopoeia standard of lactide content less than 1.5%, and glycolide content less than 0.5%. Glacial acetic acid was not detected using high performance liquid chromatography. 174.9g of refined PLGA was obtained with a yield of 87.5%.

[0058] Example 4 The raw materials were added according to the molar ratio of lactide to glycolide of 75% and 25%, the molar ratio of glycolic acid added as an initiator to the molar ratio of glycolide was 1:80, and the amount of stannous isooctanoate catalyst added was 0.75‰ of the total mass of lactide and glycolide. Under an inert environment, ring-opening polymerization was carried out at 180°C for 8h to obtain crude PLGA.

[0059] Prepare a mixed solvent of 150 L with a volume ratio of glacial acetic acid: dichloromethane = 5:95. Weigh 15 kg of crude PLGA (Mw = 65829, PDI = 1.71) and add it to 150 L of the mixed solvent. Stir at 150 rpm with an industrial anchor stirring paddle for 4 hours until it is completely dissolved.

[0060] Transport to 1200L, -6℃ cold methanol for precipitation. Filter and collect the precipitate with a flat centrifuge for about 12.5h. Then vacuum dry it in an industrial drying equipment. The vacuum degree is -101kPa, the initial drying temperature of vacuum drying is 30℃, the time is 4h, the main drying temperature is 55℃, the time is 24h, and a desiccant is used in the drying device to control the moisture. After drying, take it out and crush it into 5-10mm particles to obtain refined PLGA.

[0061] Using tetrahydrofuran as solvent, GPC was used to measure a weight average molecular weight of 68469, a molecular weight distribution index (PDI) of 1.67, which was 104.0% of the original weight average molecular weight, and the molecular weight remained consistent before and after purification. Using ICP, the tin content before and after purification was reduced from 223.6ppm to 48.7ppm, which was in line with the pharmacopoeia standard of less than 150ppm. Using high performance liquid chromatography, the lactide content was reduced from 2.80% to 0.25%, and the glycolide content was reduced from 0.18% to undetected, which was in line with the pharmacopoeia standard of lactide content less than 1.5%, and glycolide content less than 0.5%. Using high performance liquid chromatography, glacial acetic acid was not detected, and 12.3kg of refined PLGA was obtained with a yield of 82%.

[0062] Example 5 The raw materials were added according to the molar ratio of lactide to glycolide of 75% and 25%, the molar ratio of glycolic acid added as an initiator to the molar ratio of glycolide was 1:65, and the amount of stannous isooctanoate catalyst added was 0.75‰ of the total mass of lactide and glycolide. Under an inert environment, ring-opening polymerization was carried out at 180°C for 8h to obtain crude PLGA.

[0063] Prepare a mixed solvent of 2L with a volume ratio of glacial acetic acid: acetone = 1:9. Weigh 160g crude PLGA (Mw = 54480, PDI = 1.70) and add it to 2L mixed solvent. Stir at 200rpm for 2.0h and completely dissolve. Use a peristaltic pump to add dropwise to 16L of cold ethanol at -4℃ for precipitation. Filter and collect the precipitate for about 5.0h. Then vacuum dry. The vacuum degree is -101kPa, the initial drying temperature of vacuum drying is 40℃, the time is 3h, the main drying temperature is 60℃, the time is 24h, and a desiccant is used in the drying device to control the moisture. After drying, take out and crush into 5-10mm particles to obtain refined PLGA.

[0064] Using tetrahydrofuran as solvent, GPC was used to measure a weight average molecular weight of 55011, a molecular weight distribution index (PDI) of 1.68, which was 101.0% of the original weight average molecular weight, and the molecular weight remained consistent before and after purification. Using ICP, the tin content before and after purification was reduced from 210.6ppm to 24.0ppm, which met the pharmacopoeia standard of less than 150ppm. Using high performance liquid chromatography, the lactide content was reduced from 2.00% to 0.13%, and the glycolide content was reduced from 0.15% to undetected, which met the pharmacopoeia standard of lactide content less than 1.5%, and glycolide content less than 0.5%. Glacial acetic acid was not detected using high performance liquid chromatography. 139.7g of refined PLGA was obtained with a yield of 87.3%.

[0065] Table 2 Comparison of the data of purified PLGA obtained by purifying crude PLGA according to the conditions and steps of Example 5 with only different volume proportion of glacial acetic acid:

[0066] Under the same experimental conditions, 5-20% of glacial acetic acid addition has a good tin removal effect, and the molecular weight is stable and does not decrease. As the amount of glacial acetic acid added decreases, the molecular weight increases and the PDI narrows. It is surprisingly found that when the volume ratio of glacial acetic acid added is 10%-20%, the tin content of the refined PLGA obtained is a consistent minimum value, which effectively and significantly removes the tin ions in the PLGA crude product, and the molecular weight is basically the same as before purification, and the PDI narrows, indicating that the polymer is not degraded and its purification quality stability is improved. When glacial acetic acid is not within the volume ratio range, as the volume of glacial acetic acid added decreases, the tin ion removal effect is significantly weakened. As the volume of glacial acetic acid added increases, the tin removal effect is not significantly improved, the glacial acetic acid residue is high, the molecular weight gradually decreases, and the polymer degrades. Therefore, according to a series of experimental data, it can be seen that the amount of glacial acetic acid added is preferably 8-10%.

[0067] Example 6 Prepare a mixed solvent of 3 L with a volume ratio of glacial acetic acid: dichloromethane: acetone = 2:9:9. Weigh 300 g of crude PLGA (Mw = 52125, PDI = 1.71) from Example 1 and add it to the 3 L mixed solvent. Stir at 250 rpm for 3 hours until it is completely dissolved.

[0068] Use a peristaltic pump to drop into 24L of a cold precipitate containing -6℃ methanol and ethanol in a volume ratio of 1:1 for precipitation. Filter and collect the precipitate, the total time is about 7h. Then vacuum dry it. The vacuum degree is -101kPa, the initial drying temperature of vacuum drying is 30℃, the time is 3h, the main drying temperature is 60℃, the time is 24h, and a desiccant is used in the drying device to control the moisture. After drying, take it out and crush it into 5-10mm particles to obtain 268.7g of refined PLGA.

[0069] Using tetrahydrofuran as solvent, GPC measured a weight average molecular weight of 52096, a molecular weight distribution index (PDI) of 1.66, which is 99.9% of the original weight average molecular weight, and the molecular weight remained consistent before and after purification. Using ICP, the tin content before and after purification was reduced from 301.3ppm to 27.5ppm, which meets the pharmacopoeia standard of less than 150ppm. Using high-performance liquid chromatography, the lactide content was reduced from 1.80% to 0.21%, and the glycolide content was reduced from 0.15% to undetectable, which meets the pharmacopoeia standard of lactide content less than 1.5%, and glycolide content less than 0.5%. The glacial acetic acid content was not detected using high-performance liquid chromatography.

[0070] Example 7 Prepare a mixed solvent of 3 L with a volume ratio of glacial acetic acid: dichloromethane: acetone = 2:9:9. Weigh 300 g of crude PLGA (Mw = 52125, PDI = 1.71) from Example 1 and add it to the 3 L mixed solvent. Stir at 250 rpm for 3 hours until it is completely dissolved.

[0071] Use a peristaltic pump to drop into 33L, -6℃ cold methanol for precipitation. Filter and collect the precipitate, the total time is about 7h. Then vacuum dry. The vacuum degree is -101kPa, the initial drying temperature of vacuum drying is 30℃, the time is 3h, the main drying temperature is 60℃, the time is 24h, and the moisture is controlled by desiccant in the drying device. After drying, take out and crush into 5-10mm particles to obtain 274.7g of refined PLGA.

[0072] Using tetrahydrofuran as solvent, GPC measured a weight average molecular weight of 52736, a molecular weight distribution index (PDI) of 1.65, which was 101.2% of the original weight average molecular weight, and the molecular weight remained consistent before and after purification. Using ICP, the tin content before and after purification was reduced from 301.3ppm to 26.8ppm, which met the pharmacopoeia standard of less than 150ppm. Using high performance liquid chromatography, the lactide content was reduced from 1.80% to 0.14%, and the glycolide content was reduced from 0.15% to undetectable, which met the pharmacopoeia standard of lactide content less than 1.5%, and glycolide content less than 0.5%. The glacial acetic acid content was not detected using high performance liquid chromatography.

[0073] Comparative Example 1 (implemented with reference to the purification scheme disclosed in CN101939355A) Prepare 1L of a mixed solvent of lactic acid / methanol. The lactic acid content is 2mol / L. Weigh 100g of the crushed crude PLGA (Mw=52125, PDI=1.71) from Example 1 and add it to 1L of the mixed solvent. Raise the temperature to 40°C and stir at 250rpm for 6h. Remove the liquid and transfer the PLGA to 1L of methanol and stir for 1h to remove the acid. Then vacuum dry it. The vacuum drying temperature is 70°C and the time is 12h. After the PLGA is crushed, add it to 1L of methanol, raise the temperature to 70°C, stir at 250rpm for 3h, and then vacuum dry it. The vacuum degree is -101kPa and the vacuum drying temperature is 70°C for 12h.

[0074] Tetrahydrofuran was used as the solvent, and the weight average molecular weight was 31255 and the molecular weight distribution index (PDI) was 1.92 by GPC. The tin content before and after purification was reduced from 301.3 ppm to 25.7 ppm by ICP. The lactide content was reduced from 1.80% to 0.93% and the glycolide content was reduced from 0.15% to 0.08% by HPLC.

[0075] When a mixed solvent of lactic acid and methanol is used, a deacidification step is required, followed by vacuum drying. The ester bonds of PLGA are significantly hydrolyzed, and the molecular weight decreases greatly, to 60.0% of the original weight average molecular weight, indicating that the purification is not ideal.

[0076] Comparative Example 2 The method and crude PLGA (Mw=95432, PDI=1.81) were the same as those in Example 2, except that the drying method was implemented according to the scheme disclosed in CN101939355A: the vacuum degree was -101 kPa, the vacuum drying temperature was 70°C, and the time was 12 h to obtain refined PLGA.

[0077] Using tetrahydrofuran as solvent, GPC measured the weight average molecular weight to be 81150, and the molecular weight distribution index (PDI) was 1.94. Using ICP, the tin content before and after purification was reduced from 200.3ppm to 31.1ppm, which meets the pharmacopoeia standard of less than 150ppm. Using high-performance liquid chromatography, the lactide content was reduced from 1.44% to 0.33%, and the glycolide content was reduced from 0.12% to undetectable, which meets the pharmacopoeia standard of lactide content less than 1.5%, and glycolide content less than 0.5%. No glacial acetic acid was detected using high-performance liquid chromatography.

[0078] In the drying stage of Comparative Example 2, the material with residual solvent will still promote the alcoholysis and hydrolysis of the polymer ester bonds at high temperature when the solvent is not mostly removed, resulting in a slight decrease in molecular weight to 85.0% of the original weight average molecular weight, and an increase in PDI, which can easily lead to unstable polymer quality.

[0079] Comparative Example 3 (implemented with reference to the purification scheme of JP2021193160A) Weigh 50g of the crude PLGA (Mw=52125, PDI=1.71) of Example 1 and add 285g of chloroform and 5g of glacial acetic acid in sequence. Stir at 200rpm for 2h at 25℃. Use a peristaltic pump to drop into 2.0L of methanol for precipitation. Collect the precipitate by filtration. Then vacuum dry at 60℃ for 18h to obtain refined PLGA.

[0080] Tetrahydrofuran was used as solvent, and the weight average molecular weight was 40455 and the molecular weight distribution index (PDI) was 1.88 by GPC. The tin content before and after purification was reduced from 301.3ppm to 85.3ppm by ICP, and the lactide content was reduced from 1.80% to 0.61% and the glycolide content was reduced from 0.15% to 0.03% by HPLC, which met the pharmacopoeia standard of lactide content less than 1.5% and glycolide content less than 0.5%. The glacial acetic acid content was 0.01% by HPLC.

[0081] Purification of a small batch of crude PLGA, adding a small amount of glacial acetic acid, precipitation and vacuum drying can achieve a relatively ideal tin removal effect, but the molecular weight of the treated PLGA has dropped significantly, indicating that the polymer has been significantly degraded, and the PDI has become wider, which is not conducive to the quality stability of the purified PLGA. It is 77.6% of the original weight average molecular weight, and the PDI has increased, and the purification effect is not ideal. The use of chloroform is not conducive to the safety of the purification process.

[0082] Comparative Example 4 (implemented with reference to the purification scheme of JP2021193160A) The molar ratio of lactide to glycolide was 75%, and the molar ratio of glycolide to glycolide was 25%. The ratio of the molar amount of glycolic acid added as an initiator to the molar amount of glycolide was 1:78. The amount of stannous isooctanoate catalyst added was 0.90‰ of the total mass of lactide and glycolide. Under an inert environment, the crude PLGA was obtained by ring-opening polymerization at 180°C for 7h. Weigh 500g of crude PLGA (Mw = 64210, PDI = 1.68) and add 2000g of dichloromethane and 60g of lactic acid in turn. Stir at 40°C at 200rpm for 3h. Use a peristaltic pump to drop into 20L of methanol for precipitation. Filter and collect the precipitate. Then vacuum dry at 60°C for 18h to obtain refined PLGA.

[0083] Tetrahydrofuran was used as the solvent, and the weight average molecular weight was 49663 and the molecular weight distribution index (PDI) was 1.85 by GPC. The tin content before and after purification was reduced from 255.0ppm to 79.9ppm by ICP, which was in line with the pharmacopoeia standard of less than 150ppm. The lactide content was reduced from 2.16% to 0.55% by HPLC, and the glycolide content was reduced from 0.12% to undetectable, which was in line with the pharmacopoeia standard of less than 1.5% for lactide content and less than 0.5% for glycolide content.

[0084] Although the tin removal effect is ideal, when lactic acid is used in the acid reaction step at 40°C, the polymer is significantly degraded after purification, and the PDI becomes wider, which is 77.3% of the original weight average molecular weight, and the PDI is significantly increased, and the purification effect is not ideal. It is speculated that lactic acid usually contains a small amount of water, and it is difficult to obtain anhydrous lactic acid, which is easy to cause polymer hydrolysis when participating in the acid reaction. The high-temperature vacuum drying in the subsequent step further aggravates the hydrolysis of the polymer.

[0085] Comparative Example 5 (implemented with reference to the purification scheme disclosed in CN101466758A) Prepare a mixed solvent of 1L with a volume ratio of glacial acetic acid: isopropanol = 3:7. Weigh 100g of crude PLGA (Mw = 64210, PDI = 1.68) used in Comparative Example 4 and add it to 1L of mixed solvent, stir and wash at 38°C. Then remove the liquid, continue to add 1L of mixed solvent for washing, repeat the above operation, wash 10 times, and the total washing time is 48h. Then vacuum dry. The initial drying temperature of vacuum drying is 20°C, the time is 10h, the main drying temperature is 50°C, the time is 40h, and PLGA is obtained.

[0086] Using tetrahydrofuran as solvent, GPC measured the weight average molecular weight to be 51220, and the molecular weight distribution index (PDI) to be 1.83, which is 79.8% of the original weight average molecular weight, and the PDI has increased significantly. Using ICP, the tin content before and after purification was reduced from 255.0ppm to 1.9ppm. Using high performance liquid chromatography, the glacial acetic acid content was 0.85%.

[0087] The operation is complicated and uses a large amount of solvent. Although a polymer with a very low tin content can be obtained, the molecular weight stability is poor and it is very easy to degrade after long-term washing. In order to obtain refined PLGA, the subsequent monomer purification step and drying step are required, which may cause further degradation of the polymer.

[0088] Comparative Example 6 The method and crude PLGA (Mw=52125, PDI=1.71) were the same as in Example 1, except that there was no initial drying and the drying conditions were set at 55°C for 24h.

[0089] Using tetrahydrofuran as solvent, GPC measured a weight average molecular weight of 45947 and a molecular weight distribution index (PDI) of 1.93. At this time, it is 88.1% of the original weight average molecular weight, and the PDI has increased significantly. Using ICP, the tin content before and after purification was reduced from 301.3ppm to 25.0ppm, which meets the pharmacopoeia standard of less than 150ppm. Using high performance liquid chromatography, the lactide content was reduced from 1.80% to 0.18%, and the glycolide content was reduced from 0.15% to undetectable, which meets the pharmacopoeia standard of lactide content less than 1.5%, and glycolide content less than 0.5%. Using high performance liquid chromatography, the glacial acetic acid content was 0.4%.

[0090] Compared with Example 1, without initial drying, polymer partial degradation and molecular weight decrease are caused. This is because in the initial stage of drying, the amount of solvent inside the polymer is large, and the drying oven cannot reach the ultimate vacuum state in a short time. At the same time, the drying temperature is high, and high temperature promotes ester bond hydrolysis and causes the polymer molecular weight to decrease. Therefore, the sectional vacuum drying of the present invention must be adopted to avoid the above problems and ensure the stability of the polymer. The initial lower drying temperature can remove most of the solvent in a short time, so that the ultimate vacuum state is reached quickly, avoiding the problem that high temperature and vacuum degree are not enough to cause the polymer to be unstable. And the main drying is under the condition of reaching the ultimate vacuum state, and the heating further removes a small amount of solvent inside the polymer, ensuring the stability of PLGA.

[0091] The above-described embodiment is only a preferred solution of the present invention and does not limit the present invention in any form. There are other variations and modifications without exceeding the technical solution described in the claims.

Claims

1. A method for removing tin and purifying a crude PLGA product prepared by a ring-opening polymerization method, characterized in that: The following steps are involved: (1) dissolving a crude PLGA product prepared by a ring-opening polymerization method in a mixed solvent containing glacial acetic acid at room temperature to obtain a crude PLGA solution; (2) Slowly adding the crude PLGA solution to the precipitant, the volume ratio of the crude PLGA solution to the precipitant being 1:6-11, collecting the precipitate by filtration, vacuum drying and crushing the precipitate to obtain refined PLGA.

2. The tin removal and purification method according to claim 1, characterized in that: The concentration of the crude PLGA solution was 0.06-0.1 g / mL.

3. The tin removal and purification method according to claim 1, characterized in that: The mixed solvent containing glacial acetic acid consists of glacial acetic acid and a good solvent of PLGA, wherein the volume ratio of the glacial acetic acid is 5-20%.

4. The tin removal and purification method according to claim 3, characterized in that: The volume ratio of glacial acetic acid in the mixed solvent containing glacial acetic acid is 8-10%.

5. The tin removal and purification method according to claim 3, characterized in that: The good solvent for PLGA is one of dichloromethane and acetone or a combination of the two.

6. The tin removal and purification method according to claim 1, characterized in that: The volume ratio of the PLGA crude solution to the precipitant is 1:7-10.

7. The tin removal and purification method according to claim 1, characterized in that: The precipitant is methanol, ethanol or a combination of the two.

8. The tin removal and purification method according to claim 1, characterized in that: The temperature of the precipitant is controlled below -2°C.

9. The tin removal and purification method according to claim 8, characterized in that: The temperature of the precipitant is controlled at -10°C to -2°C.

10. The tin removal and purification method according to claim 1, characterized in that: Vacuum drying includes the initial drying stage and the main drying stage: Initial drying stage: temperature 30-40°C, vacuum degree -101kPa, drying for 3-4h; Main drying stage: heat to 50-60°C, vacuum degree to -101kPa, dry for 24h.