High-strength volatilization-resistant composite material as well as preparation method and application thereof
By using alkyl substituent aconitate as a plasticizer in composite materials, combined with components such as inorganic fillers and organic tin compounds, the volatility and safety of traditional plasticizers are solved, and the mechanical of the materials is improved Performance and high temperature resistance achieve a safer and sustainable plasticization effect.
Patent Information
- Application Number
- CN202310573624.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-22
- Publication Date
- 2024-11-22
AI Technical Summary
Existing plasticizers are difficult to take into account both plasticizing and safety performance in composite materials, especially traditional phenylene plasticizers are prone to volatilization, which leads to threatening human health and the environment. At the same time, bio-based environmentally friendly plasticizers are in performance and It is difficult to replace traditional plasticizers in terms of cost.
Aconitine ester containing 6-18 carbon atoms of alkyl substituents as plasticizers is used to improve compatibility with the substrate through its polar ester group and benzene-like ring structure, thereby enhancing volatility resistance and resistance. Mobility and mechanical properties, and a stable crosslinking network structure is formed through scientific proportioning and addition of components such as inorganic fillers and organic tin compounds.
It significantly improves the mechanical properties, high temperature resistance and service life of composite materials, while reducing the volatility of plasticizers, achieving a safer and more sustainable plasticization effect.
Smart Images

Figure BDA0004239297910000021 
Figure BDA0004239297910000131 
Figure BDA0004239297910000141
Abstract
Description
Technical Field
[0001] The present application relates to a high-strength, volatility-resistant composite material and a preparation method and application thereof, belonging to the technical field of plasticizer composite materials. Background Art
[0002] Plasticizer is a substance that can be added to polymer materials to improve the processability and plasticity of the materials. It is one of the most widely used and largest amount of polymer material additives. It is widely used in plastic products in construction, medical treatment, electronics, toys, etc.
[0003] Nowadays, the commonly used phthalates plasticizers are banned from use in many fields by the European Union because they are easy to migrate out of products and thus pose a threat to human health. At present, my country is also gradually restricting the use of phthalates plasticizers. As environmental protection requirements become increasingly stringent, it is urgent to find sustainable and environmentally friendly plasticizers to replace traditional phthalates plasticizers. Several bio-based environmentally friendly plasticizers such as citrate esters and epoxy vegetable oil esters have been developed one after another, but they are still lacking in competitiveness compared to traditional plasticizers with excellent plasticizing effects and low production costs. They are only used in a few special fields where traditional plasticizers have access restrictions, and cannot achieve widespread replacement.
[0004] Chinese patent CN115028814A discloses a citrate bio-based plasticizer and its preparation method and application. Under solvent or solvent-free conditions, citric acid and polymerized monomers are subjected to step-by-step ring-opening polymerization under the action of tin catalysts to obtain target polymers. However, the plasticizer molecular weight provided by the invention is relatively large, and it is in a solid state. It will affect the compatibility with the system when applied to rubber and plastic products such as PVC, causing mechanical strength to deteriorate. In addition, Chinese patent CN114112597A utilizes a milk base liquid containing phthalate plasticizer to prepare milk powder. Since the plasticizer is evenly distributed in the milk base liquid, the milk powder prepared with this, the plasticizer is also evenly distributed, thereby solving the problem of uneven distribution of plasticizers when artificially preparing plasticizer standard substances. However, phthalate plasticizers are easily volatilized from materials in PVC, causing harm to human health and the environment.
[0005] Therefore, it is difficult to balance plasticizing performance and safety performance, which is one of the main pain points in the plasticizer market. How to improve the strength and high temperature resistance of composite materials and reduce the volatility of plasticizers on the basis of improving the compatibility of plasticizers with substrates is an urgent problem to be solved. Summary of the invention
[0006] In order to solve the above problems, a high-strength volatility-resistant composite material is provided. The composite material uses aconitate ester containing an alkyl substituent with 6-18 carbon atoms as a plasticizer. The polar ester group and the benzene ring-like structure in the molecular structure of the aconitate ester both promote the compatibility of the plasticizer with the substrate, improve the volatility resistance, migration resistance, mechanical properties and high temperature resistance of the plasticizer in the substrate, and effectively extend the service life of the composite material.
[0007] According to one aspect of the present application, a high-strength, volatile-resistant composite material is provided, which comprises, by weight: 100 parts of a substrate, 5-90 parts of a plasticizer, 10-60 parts of an inorganic filler, 1-5 parts of an organic tin compound, 0.5-2 parts of a rare earth stearate, 0-2 parts of an antistatic agent, and 0.5-2 parts of a flame retardant;
[0008] The substrate is selected from at least one of cross-linked PVC resin, uncross-linked PVC resin, cross-linked nitrile rubber, and thermoplastic nitrile rubber;
[0009] The structural formula of the plasticizer is as follows:
[0010]
[0011] Wherein R1, R2, and R3 are independently selected from an alkyl group containing 6 to 18 carbon atoms;
[0012] The plasticizer is a reaction product of aconitic acid and an alkyl alcohol containing 6 to 18 carbon atoms. R1, R2 and R3 in the plasticizer can be the same substituent or different substituents. When the alkyl chain length in the plasticizer is less than 6 carbon atoms, the relative molecular mass of the plasticizer decreases, so the mobility and diffusion capabilities of the plasticizer in the substrate increase, making it easier for the plasticizer to volatilize from the substrate, resulting in poor volatility resistance of the composite material.
[0013] Therefore, when R1, R2, and R3 in the plasticizer of the present application are selected from alkyl groups containing 6-18 carbon atoms, the substituent molecular chain of the plasticizer is longer and the number of alkyl groups is also larger, which effectively increases the relative molecular mass of aconitate, making it more difficult to volatilize from a high-temperature environment, thereby improving the volatility resistance and migration resistance of the plasticizer in the substrate; at the same time, the longer alkyl chain gives the plasticizer a larger steric volume, and when it is between PVC molecular chains, it can effectively shield the interaction between PVC molecular chains, thereby enhancing the mobility of the PVC molecular chains and achieving a plasticizing effect.
[0014] The main structure of aconitate ester itself contains a double bond that cannot rotate. Similar to a benzene ring, this type of rigid main structure can play a supporting role between PVC molecular chains, further amplifying the shielding effect of the long-chain alkyl group and achieving a good plasticizing effect. Therefore, under the combined effect of the double bond structure and long-chain structure of aconitate, this type of high-boiling point aconitate long-chain ester can make the PVC material have good heat resistance and effectively plasticize PVC. The above-mentioned ratio of substrate to plasticizer can improve the plasticizing performance of the substrate and improve the stability of the substrate. Compared with the commonly used bio-based citric acid plasticizer, the addition limit of the plasticizer is also increased. The possible reason is that there is no active hydroxyl group in aconitate ester, which reduces the occurrence of side reactions, so that the addition limit of the plasticizer is increased to a certain extent, thereby improving the mechanical properties and high temperature resistance of the composite material.
[0015] If the amount of the above-mentioned plasticizer added is too much, the mechanical properties of the composite material will be reduced. The possible reason is that the aconitate plasticizer is distributed between the molecular chains of the substrate. Too much aconitate plasticizer is prone to form aggregates. Since aconitate carries an ester group, the aggregate can be made polar. Too many polar aggregates increase the defects of the substrate, and stress damage is easily generated at the aggregate, resulting in uneven distribution of the mechanical strength of the composite material; too little plasticizer cannot play a plasticizing role, and thus cannot improve the volatility resistance, migration resistance, mechanical properties and high temperature resistance of the composite material.
[0016] Preferably, the plasticizer is 30-60 parts, more preferably 50 parts.
[0017] Optionally, the substrate is selected from uncrosslinked PVC resin, and the weight average molecular weight of the uncrosslinked PVC resin is 40,000-100,000, preferably 60,000-80,000.
[0018] When the uncrosslinked PVC resin with the above molecular weight is used, the molecular chains in the PVC resin can be entangled with each other, thereby improving the toughness of the composite material and increasing the compatibility with the plasticizer. The PVC resin can also be crosslinked with the plasticizer, organic tin compound, rare earth stearate, antistatic agent and flame retardant components to form a stable crosslinked network structure, thereby improving the mechanical properties and high temperature resistance of the composite material. If the molecular weight is too high, the mechanical properties of the composite material will be reduced.
[0019] Optionally, the polydispersity index of the uncrosslinked PVC resin is 3-5, preferably 3.5-4.5;
[0020] The K value of the uncrosslinked PVC resin is 55-77.
[0021] The inventors found that when the polydispersity index of the PVC resin used is 3-5, the composite material has the best toughness and strength. This may be because when the polydispersity index of the PVC resin is 3-5, the material contains long-chain and short-chain PVC resins, and the bending of the end of the long-chain PVC resin substrate complements the short-chain PVC resin substrate, which is conducive to the insertion of the aconitate plasticizer between the molecular chains of the PVC base material, and can better react with the aconitate plasticizer containing different alkyl groups, effectively increasing the dissolution amount of the aconitate plasticizer, and can effectively combine with the resin to increase the interaction between the molecular chains, so that the prepared composite material has high toughness, high stability and plasticity, and good stability, and is not prone to problems such as phase separation.
[0022] Optionally, the plasticizer has an acid value of less than 0.1 mgKOH / g, a water content of less than 0.2%, and a purity of greater than 97%.
[0023] Preferably, the plasticizer has a purity of not less than 99% and a chromaticity of not more than 50Pt-Co.
[0024] The acid value of the plasticizer can ensure that there will not be a large amount of acidic substances in the material during use to corrode the aging material, which will affect the basic performance and internal structure of the material, so that the material has good thermal stability and migration resistance. The lower water content increases the effective ingredients of the material, and water is very easy to volatilize to the outside world, especially at high temperatures. When the water content of the plasticizer is too high, the material's volatility resistance and migration resistance will be greatly reduced, thereby reducing the thermal stability of the material. The higher the plasticizer purity, the more components that can play a plasticizing role, and the better the plasticizing effect. When the impurity content of the plasticizer increases, low-boiling impurities will volatilize and migrate to the outside world under long-term use or at high temperatures, resulting in poor product volatility resistance. At the same time, even if the impurities do not migrate outward, they will not play a plasticizing role. Therefore, at a certain amount of addition, the lower purity of the plasticizer will cause the material's volatility resistance and plasticizing effect to decrease. Therefore, the purity of the above-mentioned plasticizer can further improve the plasticization, volatility resistance and migration resistance of the plasticizer in the substrate, and improve the mechanical strength and high temperature resistance of the composite material. The chromaticity of the plasticizer is no higher than 50Pt-Co, which can reduce the coloring effect of the plasticizer on the substrate, thereby improving the controllability of the appearance of the composite material.
[0025] Optionally, the solubility of the plasticizer in 100 parts of PVC resin is greater than or equal to 50 parts, the plasticizer is liquid at 25°C, and the plasticizer is colorless, transparent or light yellow at 25°C.
[0026] The more ester groups in the plasticizer, the better the compatibility with PVC, and the stronger the ability of the plasticizer to dissolve the "crosslinking points" between PVC molecular chains (solvent effect). Although long-chain alkyl groups will weaken the polarity of the plasticizer, more ester groups make aconitate still have good compatibility and high solubility with PVC in the presence of long-chain alkyl groups.
[0027] Optionally, the inorganic filler is selected from at least one of talc, barium sulfate, calcium carbonate, titanium dioxide and clay.
[0028] The addition of inorganic filler itself can improve the thermal stability of the material, but at the same time it will increase the hardness of PVC and weaken the effect of plasticizer. The longer the alkyl chain of common plasticizer is, the more resistant to high temperature it is, but the worse it is to improve the mobility of PVC chain, making inorganic filler dispersed unevenly in PVC, so common long-chain high temperature resistant plasticizer is difficult to take into account both plasticizing effect and high temperature resistant performance. The plasticizer in this application is aconitate long chain ester, which not only has a long chain, but also has a main rigid structure containing double bonds and three ester groups. The rigid main structure and the long chain give the material a larger free volume, promote the mobility of the molecular chain, and enable the material to effectively accommodate the inorganic filler. At the same time, the uniformly distributed inorganic filler increases the contact area with the PVC material, further expands the volume between the molecular chains, and makes aconitate easier to plasticize the material. Therefore, the plasticizer in this application has a synergistic effect with the inorganic filler itself, and the plasticizing effect of aconitate will not be significantly weakened by the addition of inorganic filler, and the inorganic filler can be evenly dispersed because of aconitate to further increase the purpose of heat resistance.
[0029] Preferably, the particle size of the inorganic filler is 80-100nm. If the particle size of the inorganic filler is too large and the specific surface area is too low, the reinforcing effect of the filler on the composite material is poor and the appearance of the product will be affected; if the particle size is too small, the surface energy will increase, the particles will agglomerate seriously, and it will be difficult to completely disperse during processing, resulting in a decrease in the performance of the composite material and the appearance of particles on the surface.
[0030] The simple PVC molecular chain has poor mobility, and even if the particle size of the inorganic filler is appropriate, agglomeration will occur, resulting in an insignificant increase in the performance of the material. The plasticizer of the present application is a long-chain ester of aconitic acid, which can effectively enhance the mobility of the PVC chain, so that the three have a good dispersion effect. However, other plasticizers cannot achieve this kind of effect. Plasticizers that can provide molecular chain mobility generally have poor volatility resistance, and plasticizers with better volatility resistance have fewer ester groups or benzene rings with poor compatibility, which makes the mobility of the PVC molecular chain insufficient. Therefore, in the process of promoting the movement of the PVC molecular chain by the plasticizer of the present application, the inorganic filler in the above-mentioned particle size range of 80-100nm can achieve the best dispersion effect, and play a synergistic enhancement and plasticizing effect with the plasticizer.
[0031] Optionally, the weight ratio of the organotin compound to the rare earth stearate is (0.5-4):1, preferably (1-2):1.
[0032] Organotin compounds can effectively slow down the process of decomposing HCl during high-temperature processing of PVC, improve the processing stability and heat-resistant decomposition of PVC materials, and rare earth stearate can play the role of lubricant, promoting the product and additives to be mixed more evenly during processing. When the composite material is placed for a long time, the processing aid is easy to precipitate, which may cause the material stability to decrease. This composite material adopts an organotin compound and rare earth stearate with a weight ratio of (0.5-4): 1, which improves the dispersion performance of the composite material system and improves the mechanical properties and stability of the composite material. And the molecular weight of the organotin compound and rare earth stearate itself is large enough, and it is difficult to migrate from the material to the outside world. At the same time, its own flexible alkyl chain can further improve the effect of plasticizer shielding the PVC molecular chain under the large steric hindrance volume of aconitate, and promote the molecular chain mobility of PVC. At the same time, the two can absorb the HCl decomposed by PVC in long-term use, ensuring the long-term stability of material use.
[0033] Plasticizers exist as small molecules between the macromolecular chains of the substrate. The interaction between the plasticizer and the molecular chains of the substrate replaces the interaction between the molecular chains of the substrate, thereby increasing the free volume of the substrate. The increase in free volume improves the dispersion of organic tin compounds, inorganic fillers, rare earth stearate, antistatic agents and flame retardants in the substrate, and improves their bonding with the macromolecules of the substrate, thereby reducing the precipitation of the above components and effectively improving the mechanical properties and stability of the composite material.
[0034] Optionally, the organotin compound includes methyl tin mercaptan, di-n-butyltin maleate, di-n-octyltin dimercaptoacetate, di-n-octyltin dimethylmercaptoacetate, di-n-butyltin dodecanethiol and di-n-octyltin β-mercaptopropionate;
[0035] The rare earth stearate includes lanthanum stearate and cerium stearate.
[0036] Optionally, the antistatic agent is a quaternary ammonium salt antistatic agent;
[0037] Preferably, the quaternary ammonium salt antistatic agent is selected from at least one of stearyl trimethyl ammonium chloride, dilauryl dimethyl ammonium chloride, didecyl dimethyl ammonium chloride, dodecyl trimethyl ammonium chloride, tetradecyl trimethyl ammonium chloride and hexadecyl trimethyl ammonium chloride;
[0038] The flame retardant is selected from at least one of chlorinated paraffin, chlorinated polyethylene, tricresyl phosphate, tris(2-chloroethyl) phosphate, antimony trioxide, zinc borate, and magnesium hydroxide.
[0039] Optionally, the composite material has a volatilization loss rate of no more than 2.32% at 70° C. for 24 hours, a migration rate to PE of no more than 1.93%, and a migration rate to NR of no more than 2.02%.
[0040] Preferably, the volatilization loss rate of the composite material at 70° C. for 24 hours is not higher than 1.43%, the migration rate to PE is not higher than 1.25%, and the migration rate to NR is not higher than 1.36%.
[0041] More preferably, the composite material has a volatilization loss rate of no more than 0.84% at 70° C. for 24 hours, a migration rate to PE of no more than 0.28%, and a migration rate to NR of no more than 0.29%.
[0042] According to another aspect of the present application, a method for preparing the high-strength, volatile-resistant composite material as described in any one of the above is provided, comprising the following steps:
[0043] S1: mixing the substrate, plasticizer, organotin compound, rare earth stearate, antistatic agent and flame retardant to obtain a premix;
[0044] S2: adding the premix to a high-speed mixer, mixing at 30-80° C. for 10-60 min, and then adding the premix to a two-roll mill, mixing at 130-190° C. for 5-20 min to obtain a mixed material;
[0045] S3: placing the mixed material in a flat vulcanizer and vulcanizing it at 140-190° C. and 10-15 MPa for 5-15 min.
[0046] According to another aspect of the present application, there is provided an application of the high-strength, volatile-resistant composite material described in any one of the above items, including a home appliance housing, a printer housing, a charging gun housing, and a car taillight.
[0047] Home appliances and printers generate heat during use, so their shell materials are required to be heat-resistant and able to cope with short-circuit spontaneous combustion. Charging gun shells and car taillights need to face the dual test of "scorching sun + electric shock". The composite material prepared in this application can meet the use scenarios of the above products. In the above harsh use environment, it can still have high strength, high volatility resistance, high mobility resistance and high stability, so it can be used for a long time.
[0048] The beneficial effects of this application include but are not limited to:
[0049] 1. The high-strength, volatility-resistant composite material of the present application uses a plasticizer with an alkyl substituent having 6-18 carbon atoms, which can effectively improve the mobility of the matrix molecular chain and increase the plasticity of the material. The long-chain alkyl group makes the plasticizer have a higher boiling point and more complete contact with the matrix material, making it more difficult to volatilize from a high-temperature environment, thereby improving the volatility resistance and migration resistance of the plasticizer in the substrate.
[0050] 2. The high-strength, volatile-resistant composite material of the present application has a scientific ratio of substrate and plasticizer, which fully exerts the modification ability of the plasticizer on the matrix material. At the same time, there is a good synergistic effect between the plasticizer and the inorganic filler, thereby improving the mechanical properties and thermal stability of the composite material and extending the service life of the composite material.
[0051] 3. The high-strength, volatile-resistant composite material of the present application is added with organic tin compounds and rare earth stearate to assist in improving the uniformity of the composite material system. In addition to giving the material good resistance to thermal decomposition and demolding properties, it further improves the mechanical properties and stability of the composite material. DETAILED DESCRIPTION
[0052] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.
[0053] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.
[0054] Example 1
[0055] The present embodiment relates to a composite material and a preparation method thereof, which comprises, by weight: 100 parts of uncrosslinked PVC resin, 50 parts of tri-(2-ethylhexyl) aconitate, 30 parts of talc, 2 parts of methyltin mercaptide, 1 part of lanthanum stearate, 1.5 parts of dilauryldimethylammonium chloride and 3 parts of chlorinated paraffin, the particle size of the talc is 90 nm, the acid value of tri-(2-ethylhexyl) aconitate is 0.03 mgKOH / g, the water content is 0.04%, and the purity is 99%; the weight average molecular weight of PVC is 80,000, and the polydispersity index is 4.
[0056] The preparation method of the composite material comprises the following steps:
[0057] S1: mixing the above-mentioned uncrosslinked PVC resin, tri-(2-ethylhexyl) aconitate, methyltin mercaptan, lanthanum stearate, dilauryldimethylammonium chloride and chlorinated paraffin to obtain a premix;
[0058] S2: adding the premix to a high-speed mixer, mixing at 60° C. for 30 min, and then adding the premix to a two-roll mill, mixing at 155° C. for 15 min to obtain a mixed material;
[0059] S3: The mixed material is placed in a flat plate vulcanizing press with a press gauge pressure of 10 MPa, and vulcanized at 165° C. for 15 min.
[0060] Example 2
[0061] The present embodiment relates to a composite material and a preparation method thereof, which comprises, by weight: 100 parts of uncrosslinked PVC resin, 50 parts of n-octyl aconitate, 60 parts of barium sulfate, 5 parts of di-n-octyltin dithioacetate, 1 part of cerium stearate, 1.5 parts of stearyl trimethylammonium chloride and 3 parts of tricresyl phosphate, the particle size of the barium sulfate is 100 nm, the acid value of the n-octyl aconitate is 0.05 mgKOH / g, the water content is 0.03%, and the purity is 98%; the weight average molecular weight of PVC is 80,000, and the polydispersity index is 4. The preparation method thereof is the same as that of Example 1.
[0062] Example 3
[0063] The present embodiment relates to a composite material and a preparation method thereof, which comprises, by weight: 100 parts of uncrosslinked PVC resin, 50 parts of n-hexyl aconitate, 10 parts of calcium carbonate, 1 part of di-n-butyltin maleate, 2 parts of lanthanum stearate, 1.5 parts of dodecyltrimethylammonium chloride and 3 parts of zinc borate, the particle size of calcium carbonate is 80 nm, the acid value of n-hexyl aconitate is 0.03 mgKOH / g, the water content is 0.03%, and the purity is 98%; the weight average molecular weight of PVC is 80,000, and the polydispersity index is 4. The preparation method thereof is the same as that of Example 1.
[0064] Example 4
[0065] The difference between this embodiment and embodiment 1 is that aconitate n-dodecyl ester is used to replace aconitate tri-(2-ethylhexyl) ester, the acid value of aconitate n-dodecyl ester is 0.03 mgKOH / g, the water content is 0.04%, the purity is 97.5%, and the remaining components and preparation method are the same as those in embodiment 1.
[0066] Example 5
[0067] The difference between this embodiment and embodiment 1 is that aconitate is used to replace tri-(2-ethylhexyl) aconitate, the acid value of aconitate is 0.04 mgKOH / g, the water content is 0.05%, the purity is 98.5%, and the other components and preparation method are the same as those in embodiment 1.
[0068] Example 6
[0069] The difference between this embodiment and embodiment 1 is that dihexyl-isooctyl aconitate is used, in which two substituents in R1, R2 and R3 are hexyl groups and one substituent is isooctyl group, and the acid value is 0.05 mgKOH / g, the water content is 0.03%, the purity is 98.5%, and the other components and preparation method are the same as those in embodiment 1.
[0070] Example 7
[0071] The difference between this embodiment and embodiment 1 is that tri-(2-ethylhexyl) aconitate and n-hexyl aconitate in a weight ratio of 1:1 are used, the parameters of tri-(2-ethylhexyl) aconitate and n-hexyl aconitate are the same as those in embodiment 1 and embodiment 3, and the remaining components and preparation method are the same as those in embodiment 1.
[0072] Example 8
[0073] The difference between this embodiment and embodiment 1 is that the weight average molecular weight of PVC is 120,000, and the other components and preparation method are the same as those in embodiment 1.
[0074] Example 9
[0075] The difference between this embodiment and embodiment 1 is that the weight average molecular weight of PVC is 30,000, and the other components and preparation method are the same as those in embodiment 1.
[0076] Example 10
[0077] The difference between this embodiment and embodiment 1 is that the polydispersity index of PVC is 5.5, and the other components and preparation method are the same as those in embodiment 1.
[0078] Embodiment 11
[0079] The difference between this embodiment and embodiment 1 is that the polydispersity index of PVC is 2.5, and the other components and preparation method are the same as those in embodiment 1.
[0080] Example 12
[0081] The difference between this embodiment and embodiment 1 is that thermoplastic nitrile rubber is used to replace the uncrosslinked PVC resin, the molecular weight of the thermoplastic nitrile rubber is 700,000, and the other components and preparation method are the same as those in embodiment 1.
[0082] Embodiment 13
[0083] The difference between this embodiment and embodiment 1 is that the acid value of tri-(2-ethylhexyl) aconitate is 0.12 mgKOH / g, and the other components and preparation method are the same as those in embodiment 1.
[0084] Embodiment 14
[0085] The difference between this embodiment and embodiment 1 is that the water content of tri-(2-ethylhexyl) aconitate is 4%, and the other components and preparation method are the same as those in embodiment 1.
[0086] Embodiment 15
[0087] The difference between this embodiment and embodiment 1 is that the purity of tri-(2-ethylhexyl) aconitate is 95%, and the other components and preparation method are the same as those in embodiment 1.
[0088] Example 16
[0089] The difference between this embodiment and embodiment 1 is that 2.5 parts of methyltin mercaptide and 0.5 parts of lanthanum stearate are used, and the remaining components and preparation method are the same as those in embodiment 1.
[0090] Embodiment 17
[0091] The difference between this embodiment and embodiment 1 is that di-n-butyltin dodecanethiol is used to replace methyltin mercaptan, and the other components and preparation method are the same as those in embodiment 1.
[0092] Embodiment 18
[0093] The difference between this embodiment and embodiment 1 is that cerium stearate is used to replace lanthanum stearate, and the other components and preparation method are the same as those in embodiment 1.
[0094] Embodiment 19
[0095] The difference between this embodiment and embodiment 1 is that dilauryl dimethyl ammonium chloride is not added, and the remaining components and preparation method are the same as those in embodiment 1.
[0096] Embodiment 20
[0097] The difference between this embodiment and embodiment 1 is that chlorinated polyethylene is used to replace chlorinated paraffin, and the other components and preparation method are the same as those in embodiment 1.
[0098] Embodiment 21
[0099] The difference between this embodiment and embodiment 1 is that 5 parts of tri-(2-ethylhexyl) aconitate are added, and the other components and preparation method are the same as those in embodiment 1.
[0100] Embodiment 22
[0101] The difference between this embodiment and embodiment 1 is that the particle size of talcum powder is 150 nm, and the other components and preparation method are the same as those in embodiment 1.
[0102] Embodiment 23
[0103] The difference between this embodiment and embodiment 1 is that the particle size of talcum powder is 20 nm, and the other components and preparation method are the same as those in embodiment 1.
[0104] Comparative Example 1
[0105] The difference between this comparative example and Example 1 is that dioctyl phthalate is used to replace tri-(2-ethylhexyl) aconitate, and the other components and preparation method are the same as those in Example 1.
[0106] Comparative Example 2
[0107] The difference between this comparative example and Example 1 is that dioctyl terephthalate is used to replace tri-(2-ethylhexyl) aconitate, and the other components and preparation method are the same as those in Example 1.
[0108] Comparative Example 3
[0109] The difference between this comparative example and Example 1 is that dioctyl adipate is used to replace tri-(2-ethylhexyl) aconitate, and the other components and preparation method are the same as those in Example 1.
[0110] Comparative Example 4
[0111] The difference between this comparative example and Example 1 is that tributyl citrate is used to replace tri-(2-ethylhexyl) aconitate, and the other components and preparation method are the same as those in Example 1.
[0112] Comparative Example 5
[0113] The difference between this comparative example and Example 1 is that aconitate tripentyl ester is used to replace aconitate tri-(2-ethylhexyl) ester, the acid value of the aconitate tripentyl ester is 0.07 mgKOH / g, the water content is 0.07%, the purity is 97.5%, and the other components and preparation method are the same as those in Example 1.
[0114] Comparative Example 6
[0115] The difference between this comparative example and Example 1 is that calcium stearate is used to replace lanthanum stearate, and the other components and preparation method are the same as those in Example 1.
[0116] Comparative Example 7
[0117] The difference between this comparative example and Example 1 is that talc is not contained, and the other components and preparation method are the same as those of Example 1.
[0118] Test Case
[0119] The composite materials prepared in the above examples and comparative examples were tested for performance, and the results are shown in Tables 1 and 2. The test methods are as follows:
[0120] 1. Hardness: According to GB / T531-2008 "Indentation hardness test method, Shore hardness tester method" standard, make specimens and test them. Select 3 points for each group of specimens, measure each point once, and take the median value.
[0121] 2.100% tensile stress, elongation at break, elastic modulus: in accordance with GB / T1040-2006 "Plastic Tensile Properties Test", the stretching speed is 50mm / min, the temperature is 25℃.
[0122] 3. Compatibility: The water price method is used for testing. Since water molecules are polar, the compatibility of plasticizers with water can characterize the compatibility of plasticizers with polar materials (PVC, PLA and nitrile rubber). When a certain plasticizer has good compatibility with water, it has good compatibility with PVC, and vice versa. In the experiment, 2.5g of plasticizer and 25g of acetone were added to a beaker, and titrated with a burette filled with deionized water, stirring while titrating until turbidity appeared, and the volume of deionized water consumed was recorded.
[0123] 4. Glass transition temperature (T g ): The glass transition temperature was tested by a dynamic mechanical analyzer. The test conditions were: nitrogen as the carrier gas, the test temperature range was -40 to 80°C, the heating rate was 3°C / min, and the frequency was 1 Hz.
[0124] 5. Volatilization loss rate: The test is carried out in accordance with HG / T 4458-2012 "Determination of plasticizer loss in plastics - Activated carbon method", the test temperature is 70°C, and the test time is 24h.
[0125] 6. Migration rate: The test is conducted in accordance with HG / T 4458-2012 “Determination of Migration of Plasticizers in Plastics”. The test temperature is 50°C and the test time is 48 hours. The absorbent sheet is made of polyethylene (PE) without additives and standard natural rubber (NR).
[0126] Table 1
[0127]
[0128]
[0129]
[0130] Table 2
[0131]
[0132]
[0133] According to the contents of Table 1 and Table 2, in this composite system, the various additives, especially the aconitate ester and other additives, play a good synergistic role, not just a single role in one aspect. The change in the ratio of the components between the additives has a certain influence on the performance of the material. For the long-chain aconitate ester, compared with other plasticizers, the long-chain aconitate ester has good volatility resistance and migration resistance.
[0134] According to the comparison between Examples 8-11 and Example 1, the molecular weight and polydispersity index of the PVC resin can affect the compatibility of the plasticizer with the PVC resin, and affect the synergistic effect of the plasticizer with the inorganic filler, so that the toughness, volatility resistance and migration resistance of the composite material are reduced.
[0135] According to the comparison between Examples 13-15 and Example 1, the acid value, water content and purity of the plasticizer will affect the plasticizing effect of the plasticizer on the PVC resin, and affect the mobility of the PVC molecular chain, resulting in poor dispersibility of the inorganic filler in the PVC molecular chain, which reduces the mechanical properties of the composite material. The acid value, water content and purity of the plasticizer will also affect the volatility resistance, migration resistance and thermal stability of the material.
[0136] According to the comparison between Examples 16-20 and Example 1, the type of organotin compound, the type of rare earth stearate, the type of flame retardant, the weight ratio of organotin compound and rare earth stearate, and the number of antistatic agents added will affect the synergistic effect of the above substances with inorganic fillers and plasticizers, thereby affecting the mechanical properties, volatility resistance and migration resistance of the composite material. According to the comparison between Comparative Example 6 and Example 1, when calcium stearate is used to replace rare earth stearate, calcium stearate cannot have a synergistic effect with inorganic fillers and plasticizers, and all aspects of the performance of the composite material are reduced.
[0137] According to the comparison of Examples 21-23, Comparative Example 7 and Example 1, the inorganic filler of the present application can be evenly dispersed in the composite material under the action of the plasticizer, and has a synergistic plasticizing effect with the plasticizer. The particle size of the inorganic filler will also affect its dispersibility in the composite material and its synergistic effect with the plasticizer. When the particle size is less than 80nm or greater than 100nm, the reinforcing effect on the composite material is weakened. If the particle size is too small, agglomeration is likely to occur; if the particle size is too large, stress concentration is likely to occur, and cracks are likely to occur after long-term use, and various performances of the composite material are reduced.
[0138] According to the comparison between Comparative Examples 1-5 and Example 1, it can be seen that the use of other types of plasticizers has a poor effect on improving the mobility of PVC molecular chains, thereby making the dispersibility of inorganic fillers in PVC molecular chains worse, and the synergistic effect of plasticizers and inorganic fillers is poor, reducing the plasticizing effect of plasticizers on composite materials.
[0139] The above is only the embodiment of the present application, and the protection scope of the present application is not limited by these specific embodiments, but is determined by the claims of the present application. For those skilled in the art, the present application can have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the technical ideas and principles of the present application should be included in the protection scope of the present application.
Claims
1. A high-strength, volatile-resistant composite material, characterized in that: The composition comprises, by weight: 100 parts of a base material, 5-90 parts of a plasticizer, 10-60 parts of an inorganic filler, 1-5 parts of an organic tin compound, 0.5-2 parts of rare earth stearate, 0-2 parts of an antistatic agent and 0.5-2 parts of a flame retardant; The substrate is selected from at least one of cross-linked PVC resin, uncross-linked PVC resin, cross-linked nitrile rubber, and thermoplastic nitrile rubber; The structural formula of the plasticizer is as follows: Wherein R1, R2, and R3 are independently selected from an alkyl group containing 6 to 18 carbon atoms; The volatilization loss rate of the plasticizer in the composite material at 70° C. for 24 hours is no more than 2.32%.
2. The high-strength, volatile-resistant composite material according to claim 1, characterized in that: The substrate is selected from uncrosslinked PVC resin, and the weight average molecular weight of the uncrosslinked PVC resin is 40,000-100,000, preferably 60,000-80,000.
3. The high-strength, volatile-resistant composite material according to claim 2, characterized in that: The polydispersity index of the uncrosslinked PVC resin is 3-5, preferably 3.5-4.5; The K value of the uncrosslinked PVC resin is 55-77.
4. The high-strength, volatile-resistant composite material according to claim 1, characterized in that: The plasticizer has an acid value of less than 0.1 mgKOH / g, a water content of less than 0.2%, and a purity of more than 97%.
5. The high-strength, volatile-resistant composite material according to claim 1, characterized in that: The weight ratio of the organotin compound to the rare earth stearate is (0.5-4):1, preferably (1-2):
1.
6. The high-strength, volatile-resistant composite material according to claim 1, characterized in that: The organotin compounds include methyl tin mercaptan, di-n-butyltin maleate, di-n-octyltin dimercaptoacetate, di-n-octyltin dimethylmercaptoacetate, di-n-butyltin dodecanethiol and di-n-octyltin β-mercaptopropionate; The rare earth stearate includes lanthanum stearate and cerium stearate.
7. The high-strength, volatile-resistant composite material according to claim 1, characterized in that: The antistatic agent is a quaternary ammonium salt antistatic agent; Preferably, the quaternary ammonium salt antistatic agent is selected from at least one of stearyl trimethyl ammonium chloride, dilauryl dimethyl ammonium chloride, didecyl dimethyl ammonium chloride, dodecyl trimethyl ammonium chloride, tetradecyl trimethyl ammonium chloride and hexadecyl trimethyl ammonium chloride; The flame retardant is selected from at least one of chlorinated paraffin, chlorinated polyethylene, tricresyl phosphate, tris(2-chloroethyl) phosphate, antimony trioxide, zinc borate, and magnesium hydroxide.
8. The high-strength, volatile-resistant composite material according to claim 1, characterized in that: The inorganic filler is selected from at least one of talc, barium sulfate, calcium carbonate, titanium dioxide and clay.
9. The method for preparing the high-strength and volatile-resistant composite material according to any one of claims 1 to 8, characterized in that: The steps include: S1: mixing the substrate, plasticizer, organotin compound, rare earth stearate, antistatic agent and flame retardant to obtain a premix; S2: adding the premix to a high-speed mixer, mixing at 30-80° C. for 10-60 min, and then adding the premix to a two-roll mill, mixing at 130-190° C. for 5-20 min to obtain a mixed material; S3: placing the mixed material in a flat vulcanizer and vulcanizing it at 140-190° C. and 10-15 MPa for 5-15 min.
10. Use of the high-strength, volatile-resistant composite material according to any one of claims 1 to 8, characterized in that: Including home appliance housings, printer housings, charging gun housings and car taillights.
Citation Information
Patent Citations
Polyvinyl chloride sheath material and application thereof
CN111849088A
Aconitate polyvinyl chloride plasticizer, and preparation method and application thereof
CN113817223A
Plasticizer composition, and vinylchloride resin composition comprising same
WO2023085815A1
Cited By
Bio-based trans-aconitate, preparation method therefor and use thereof
EP4715056A1
Bio-based trans-aconitate, preparation method therefor and use thereof
WO2024235233A1