Low-temperature low-modulus high-initial-strength high-final-strength two-component polyurethane structural adhesive as well as preparation method and application thereof
By reasonably selecting the combination of plasticizer and polyol in two-component polyurethane structural glue, combining dimeric acid polyester polyol modified isocyanate prepolymer, the problems of low temperature modulus and aging resistance are solved, and low temperature and low temperature are achieved The combination of modulus, high initial strength and excellent aging resistance ensures the safety and bonding stability of the glass.
Patent Information
- Application Number
- CN202411130595.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-22
AI Technical Summary
The modulus of the existing two-component polyurethane structural adhesives increased sharply at low temperatures, resulting in glass rupture problems. The initial strength generation time is long and the aging resistance is poor, making it difficult to have both low temperature modulus, high initial strength and excellent aging resistance. .
By rationally selecting plasticizers, combining the combination of different polyols, designing and introducing dimeric acid polyester polyol modified isocyanate prepolymers, reducing the low-temperature modulus, while improving the initial and terminal bonding strength and improving moisture and heat resistance.
Two-component polyurethane structural adhesive with low temperature and low modulus, high initial strength, high final strength, humidity and heat aging resistance and cold and heat impact resistance, meets customers' bonding requirements, and reduces the DMA modulus of low temperature in -40℃ to below 1100MPa. The DMA modulus at room temperature dropped to below 500MPa, the initial strength remained above 5 minutes, the interface shear strength reached above 8MPa, and the cold and hot cycles did not degummize and the glass did not break after 300 times.
Smart Images

Figure QLYQS_1 
Figure QLYQS_2 
Figure QLYQS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the field of adhesives, and specifically relates to a low-temperature, low-modulus, high initial strength and high final strength two-component polyurethane structural adhesive, and a preparation method and application thereof. Background Art
[0002] In recent years, with the development and gradual popularization of automobiles, in addition to the improvement of performance and functions, consumers are also very concerned about the appearance design of automobiles. Therefore, at this stage, the appearance design of traditional automobiles is becoming more and more fashionable and personalized, and more and more models adopt frameless window design.
[0003] Compared with the traditional frame window design, the frameless window design generally uses a two-component polyurethane structural adhesive for fixing. Conventional two-component polyurethane structural adhesive has a medium modulus at room temperature, but the modulus rises sharply at low temperatures (usually -40°C), which causes the stress between the polyurethane structural adhesive and the glass to rise sharply at low temperatures, and it is easy to cause problems such as glass breakage. Conventional two-component polyurethane structural adhesives take a long time (usually more than 7 days) to cure completely. In order to speed up the production cycle and improve efficiency, customers are particularly concerned about the initial strength generation of two-component polyurethane structural adhesives. For low-modulus two-component polyurethane structural adhesives, it is more difficult to improve the initial strength. In addition, conventional two-component polyurethane structural adhesives have poor aging resistance (resistance to moisture and heat aging and resistance to cold and heat shock). In order to improve the low-temperature modulus performance of existing two-component polyurethane structural adhesives, plasticizers are generally added to the two-component polyurethane structural adhesives. Although this method can reduce the low-temperature modulus to a certain extent, the introduction of plasticizers will actually greatly reduce the initial bonding strength (initial strength), final bonding strength (final strength), moisture and heat aging resistance and thermal shock resistance of the two-component polyurethane structural adhesive. In view of this, how to obtain a two-component polyurethane structural adhesive with low low-temperature modulus, high initial bonding strength and excellent aging resistance (moisture and heat aging resistance and thermal shock resistance) has become an urgent problem to be solved, so as to provide downstream automotive customers and consumers with safer and more reliable solutions. Summary of the invention
[0004] The first object of the present invention is to provide a new two-component polyurethane structural adhesive, which has low low-temperature modulus, high initial strength and high final strength, and excellent aging resistance (resistance to wet and hot aging and resistance to cold and hot shock) properties.
[0005] Specifically, the two-component polyurethane structural adhesive provided by the present invention contains component A and component B in a volume ratio of 1:(0.25-4); the component A contains polyester polyol I, polyether polyol I, castor oil polyol I and plasticizer I in a mass ratio of 100:(1-9000):(1-9000):(1-3000); the component B contains polyisocyanate I, polyurethane prepolymer and plasticizer II in a mass ratio of 100:(50-8500):(10-3000); the polyurethane prepolymer The polyurethane prepolymer is obtained by reacting a polyol mixture with polyisocyanate II, wherein the polyol mixture contains dimer acid polyester polyol and other polyols at the same time, wherein the other polyols are selected from at least one of polyester polyol II, polyether polyol II and castor oil polyol II other than dimer acid polyester polyol; the NCO content in the polyurethane prepolymer is 5-23wt%; and the plasticizer I and plasticizer II are independently selected from at least one of phthalate esters, aliphatic diacid esters, benzoic acid glycol esters and phosphate ester plasticizers.
[0006] In a preferred embodiment,
[0007] The A component contains the following raw materials in the A component in percentage by mass:
[0008]
[0009] The B component contains the following raw materials in the B component in percentage by mass:
[0010]
[0011]
[0012] In a preferred embodiment, the polyurethane prepolymer is prepared according to the following method: vacuum dehydrating a polyol mixture at 100-120°C to a water content of less than 300ppm, reducing the temperature of the dehydrated polyol mixture to 45-55°C, adding polyisocyanate II, and reacting while stirring at 78-82°C to achieve an NCO content of 5-23wt% under inert gas protection, and then cooling to obtain a polyurethane prepolymer.
[0013] In a preferred embodiment, the mass ratio of dimer acid polyester polyol to other polyols in the polyol mixture is (0.1-10):1.
[0014] In a preferred embodiment, the dimer acid structural unit in the dimer acid polyester polyol is at least one of a polyoleic acid structural unit, a polylinoleic acid structural unit, a polylinolenic acid structural unit and a polyarachidonic acid structural unit.
[0015] In a preferred embodiment, the number average molecular weight of the dimer acid polyester polyol is 1000-3000.
[0016] In a preferred embodiment, the molar ratio of the total content of hydroxyl groups to the total content of isocyanate groups in the two-component polyurethane structural adhesive is 1:(1-1.5).
[0017] In a preferred embodiment, the number average molecular weight of the polyester polyol I and the polyester polyol II in the component A is independently 500-4000, and the functionality is independently 2-4.
[0018] In a preferred embodiment, the polyether polyol I and the polyether polyol II are each independently selected from at least one of polyoxypropylene diol having a number average molecular weight of 100-5000, polyoxypropylene triol having a number average molecular weight of 250-6000, polytetrahydrofuran diol having a number average molecular weight of 500-4000, bisphenol A modified polyether polyol having a number average molecular weight of 500-4000 and polyoxyethylene polyol having a number average molecular weight of 500-4000.
[0019] In a preferred embodiment, the number average molecular weight of the castor oil polyol I and the castor oil polyol II are independently 400-5000, and the functionality is independently 2-4.
[0020] In a preferred embodiment, the polyisocyanate I and the polyisocyanate II are each independently selected from at least one of a mixture of diphenylmethane-4,4'-diisocyanate and diphenylmethane-2,2'-diisocyanate and / or diphenylmethane-2,4'-diisocyanate, carbodiimide-modified MDI, polyether-modified MDI, polymethylene polyphenyl polyisocyanate, 4,4'-dicycloethylmethane diisocyanate and isophorone diisocyanate.
[0021] In a preferred embodiment, the filler I and filler II are each independently selected from at least one of aluminum hydroxide, aluminum oxide, calcium carbonate, talcum powder, quartz powder, mica powder, titanium dioxide, white carbon black, bentonite and carbon black.
[0022] In a preferred embodiment, the molecular sieve I and molecular sieve II are each independently selected from at least one of mordenite, Y zeolite, ZSM-5 molecular sieve, MCM-22 molecular sieve, MCM-56 molecular sieve and Beta molecular sieve.
[0023] In a preferred embodiment, the auxiliary agent I is selected from at least one of color paste, defoamer, dewatering agent, rheological agent, leveling agent, wetting agent, coupling agent, stabilizer and catalyst.
[0024] In a preferred embodiment, the auxiliary agent II is selected from at least one of a defoamer, a stabilizer, an inhibitor, a leveling agent, a leveling agent and a thixotropic agent.
[0025] The second object of the present invention is to provide a method for preparing the above-mentioned two-component polyurethane structural adhesive, which method comprises the following steps:
[0026] Preparation of component A: Mix all the raw materials in component A evenly and then remove the vacuum to obtain component A;
[0027] Preparation of component B: Mix the raw materials in component B evenly and then de-vacuum to obtain component B.
[0028] The third object of the present invention is to provide the application of the above-mentioned two-component polyurethane structural adhesive in the fixation of glass on frameless windows of new energy vehicles and structural bonding at low temperatures.
[0029] The key of the present invention is to achieve the purpose of high initial strength by adopting a combination design of different polyols and matching plasticizers in component A under the premise of reasonably selecting the modulus reduction of plasticizer, especially the modulus at low temperature. At the same time, a specific polyurethane prepolymer is introduced into component B, mainly by introducing dimer acid polyester polyol modified isocyanate prepolymer. Since dimer acid polyester polyol has a long carbon chain structure, it can provide excellent wettability, thereby improving the bonding performance of the two-component polyurethane structural adhesive to various substrates, and finally achieving high final strength and cohesive failure form; in addition, dimer acid polyester polyol also has an ultra-long branched chain segment, so that the prepared polyurethane prepolymer has excellent hydrophobicity, can give the structural adhesive excellent water resistance, and improve the resistance to wet heat aging. The two-component polyurethane structural adhesive provided by the present invention can resist the influence of the introduction of plasticizers on strength and aging resistance, and achieve the purpose of reducing the low-temperature modulus of the two-component polyurethane structural adhesive and improving the resistance to cold and hot shocks. That is, the two-component polyurethane structural adhesive provided by the present invention has the characteristics of low modulus at low temperature, high initial strength and final strength, excellent resistance to moisture and heat aging and resistance to cold and hot shock, etc. Specifically, on the basis of meeting the customer's requirements for bonding, the low-temperature DMA modulus at -40°C is reduced from 5000MPa of the traditional polyurethane structural adhesive to below 1100MPa, and the DMA modulus at room temperature is reduced to below 500MPa; in terms of initial strength, the open time is maintained for more than 5 minutes, and the interface shear strength after heating at 80°C for 5 minutes can reach more than 0.81MPa, the final interface shear strength reaches more than 8MPa, and all interface failures are cohesive failures; it has excellent bonding performance under high temperature and high humidity (the bonding strength after double 85 aging for 1000h is more than 5MPa), and there is no debonding and glass cracking after 300 cold and hot cycles. DETAILED DESCRIPTION
[0030] The two-component polyurethane structural adhesive provided by the present invention contains component A and component B. The volume ratio of component A to component B is 1:(0.25-4), such as 1:0.25, 1:0.5, 1:0.75, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4 or any value therebetween.
[0031] In the present invention, the component A contains polyester polyol I, polyether polyol I, castor oil polyol I and plasticizer I. Based on the total content of polyester polyol I as 100 parts by weight, the content of polyether polyol I and castor oil polyol I is independently 1-9000 parts by weight, such as 1, 5, 10, 50, 100, 200, 300, 400, 500, 600, 700, 800, 900, 1000, 1500, 2000, 2500, 3000, 3500, 4000, 4500, 5000, 5500, 6000, 6500, , 7000, 7500, 8000, 8500, 9000 parts by weight or any value therebetween; the content of the plasticizer I is 1-3000 parts by weight, such as 1, 5, 10, 50, 100, 200, 300, 400, 500, 600, 700, 800, 900, 1000, 1200, 1500, 1800, 2000, 2200, 2500, 2800, 3000 parts by weight or any value therebetween. In addition, the component A may also selectively contain at least one of filler I, molecular sieve I, auxiliary agent I and fumed silica I according to actual conditions. Based on the total content of polyester polyol I as 100 parts by weight, the content of filler I is preferably 1-8000 parts by weight, such as 1, 5, 10, 50, 100, 200, 300, 400, 500, 600, 700, 800, 900, 1000, 1500, 2000, 2500, 3000, 3500, 4000, 4500, 5000, 5500, 6000, 6500, 7000, 7500, 8000 parts by weight or any value therebetween; the content of molecular sieve I is preferably 1-1500 parts by weight, such as 1, 5, 10, 20, 30, 40 0, 50, 60, 70, 80, 90, 100, 200, 500, 800, 1000, 1200, 1500 parts by weight or any value therebetween; the content of the auxiliary agent I is preferably 1-1000 parts by weight, such as 1, 5, 10, 50, 100, 200, 300, 400, 500, 600, 700, 800, 900, 1000 parts by weight or any value therebetween; the content of the fumed silica I is preferably 1-500 parts by weight, such as 1, 5, 10, 50, 100, 200, 300, 400, 500 parts by weight or any value therebetween. In the most preferred embodiment, the component A contains the following raw materials in terms of mass percentage in component A: polyester polyol I 1-90%, polyether polyol I 1-90%, castor oil polyol I 1-90%, plasticizer I 1-30%, filler I 1-80%, molecular sieve I 1-15%, additive I 0.1-10%, and fumed silica I 1-5%.
[0032] In the present invention, the B component contains polyisocyanate I, polyurethane prepolymer and plasticizer II. Based on 100 parts by weight of polyisocyanate I, the content of the polyurethane prepolymer is 50-8500 parts by weight, such as 50, 100, 200, 300, 400, 500, 600, 700, 800, 900, 1000, 1200, 1500, 1800, 2000, 2500, 3000, 3500, 4000, 4500, 5000, 5500, 6000, 6500, 7000, 7500, 8000, 8500 parts by weight or any value therebetween; the content of the plasticizer II is 10-3000 parts by weight, such as 10, 50, 100, 200, 300, 400, 500, 600, 700, 800, 900, 1000, 1200, 1500, 1800, 2000, 2200, 2500, 2800, 3000 parts by weight or any value therebetween. In addition, the component B may also selectively contain at least one of filler II, molecular sieve II, auxiliary agent II and fumed silica II according to actual conditions. Based on 100 parts by weight of polyisocyanate I, the content of filler II is preferably 10-8000 parts by weight, such as 10, 50, 100, 300, 500, 800, 1000, 1500, 2000, 2500, 3000, 3500, 4000, 4500, 5000, 5500, 6000, 6500, 7000, 7500, 8000 parts by weight or any value therebetween; the content of molecular sieve II is preferably 10-1500 parts by weight, such as 10, 50, 100, 300, 500, 800, 1000, 1500 parts by weight or any value therebetween; the content of the auxiliary agent II is preferably 10-1000 parts by weight, such as 10, 30, 50, 100, 200, 300, 400, 500, 600, 700, 800, 900, 1000 parts by weight or any value therebetween; the content of the fumed silica II is preferably 1-500 parts by weight, such as 1, 5, 10, 50, 100, 200, 300, 400, 500 parts by weight or any value therebetween. In the most preferred embodiment, the B component includes the following raw materials in terms of mass percentage in the B component: polyisocyanate I 1-10%, polyurethane prepolymer 5-85%, plasticizer II 1-30%, filler II 1-80%, molecular sieve II 1-15%, additive II 1-10%, and fumed silica II 1-5%.
[0033] In the present invention, the NCO content in the polyurethane prepolymer is 5-23wt%, such as 5wt%, 8wt%, 10wt%, 12wt%, 15wt%, 18wt%, 20wt%, 22wt%, 23wt% or any value therebetween. Wherein, the NCO content is determined by the following method: weigh about mg of sample in a stoppered conical flask, add 25mL of anhydrous toluene, cover the bottle stopper, and heat on a heating plate to dissolve quickly; use a pipette to draw 25mL of di-n-butylamine toluene solution (0.1mol / L), cover the stopper and shake to dissolve fully, add 20mL of isopropanol, insert electrodes and titration head, set titration parameters, and titrate with 0.5852mol / L hydrochloric acid standard solution (Vs); repeat the above operation without adding sample to determine the sample blank (V0); according to W NCO =(V0-Vs)*0.5852*42 / (1000m)*100% to calculate the NCO content. The polyurethane prepolymer is obtained by reacting a polyol mixture containing dimer acid polyester polyol and other polyols with polyisocyanate II, wherein the other polyols are selected from at least one of polyester polyol II, polyether polyol II and castor oil polyol II. When the polyol mixture contains polyester polyol II, polyether polyol II and castor oil polyol II at the same time, it is more conducive to improving the bonding performance and heat and humidity aging resistance. The reaction method is preferably as follows: vacuum dehydrating the polyol mixture at 100-120°C to a water content of less than 300ppm, lowering the temperature of the dehydrated polyol to 45-55°C, and then adding isocyanate, and under the protection of inert gas, heating to 78-82°C while stirring to react until the NCO content reaches 5-23wt%, and then cooling to obtain the polyurethane prepolymer. The mass ratio of the dimer acid polyester polyol to the other polyols in the polyol mixture is preferably (0.1-10):1, such as 0.1:1, 0.5:1, 1:1, 2:1, 4:1, 6:1, 8:1, 10:1 or any value therebetween.
[0034] In the present invention, term " dimer acid polyester polyol " refers to the alcohol compound obtained by condensation reaction of dimer acid and polyol and other acids except dimer acid optionally.Wherein, described dimer acid can be prepared by existing unsaturated fatty acid separately through polymerization reaction.Wherein, described unsaturated fatty acid can be monounsaturated fatty acid, can also be polyunsaturated fatty acid, for example, preferably selected from at least one of oleic acid, linoleic acid, linolenic acid and arachidonic acid.Correspondingly, the dimer acid structural unit in described dimer acid polyester polyol is preferably selected from at least one of polyoleic acid structural unit, polylinoleic acid structural unit, polylinolenic acid structural unit and polyarachidonic acid structural unit.In addition, the number average molecular weight of described dimer acid polyester polyol is preferably 1000-3000, such as 1000,1200,1400,1600,1800,2000,2200,2400,2600,2800,3000 or any value therebetween.
[0035] In the present invention, the plasticizer I and the plasticizer II are independently selected from at least one of phthalate, aliphatic diacid, benzoic acid glycol ester and phosphate plasticizer. Specific examples of the phthalate include, but are not limited to, at least one of dimethyl phthalate (DMP), diethyl phthalate (DEP), di-n-butyl phthalate (DBP), diisobutyl phthalate (DIBP), (2-ethylhexyl) phthalate (DEHP), butyl benzyl phthalate (BBP), diisononyl phthalate (DINP), diisodecyl phthalate (DIDP) and dioctyl phthalate (DNOP). Specific examples of the aliphatic diacid include, but are not limited to, at least one of dimethyl adipate, diisopropyl adipate, diisononyl cyclohexane-1,2-dicarboxylate and dioctyl azelate. Specific examples of the benzoic acid glycol ester include, but are not limited to, at least one of diethylene glycol, triethylene glycol and dipropylene glycol. Specific examples of the phosphate ester plasticizer include, but are not limited to, at least one of triphenyl phosphate, tricresyl phosphate, diphenyl isooctyl phosphate, triethyl phosphate, tributyl phosphate and trioctyl phosphate.
[0036] In the present invention, the molar ratio of the total content of hydroxyl groups to the total content of isocyanate groups in the two-component polyurethane structural adhesive is preferably 1:(1-1.5), such as 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1:1.5 or any value therebetween.
[0037] In the present invention, the number average molecular weight of the polyester polyol I and the polyester polyol II is preferably independently 500-4000, such as 500, 800, 1000, 1200, 1500, 1800, 2000, 2200, 2500, 2800, 3000, 3200, 3500, 3800, 4000 or any value therebetween; the functionality is preferably independently 2-4, such as 2, 3 or 4. The polyester polyol I and the polyester polyol II are preferably selected from polycaprolactone polyol and / or polycarbonate polyol.
[0038] In the present invention, the polyether polyol I and the polyether polyol II are preferably independently selected from at least one of polyoxypropylene diol, polyoxypropylene triol, polytetrahydrofuran diol, bisphenol A modified polyether polyol and polyoxyethylene polyol. The number average molecular weight of the polyoxypropylene diol is preferably 100-5000, such as 100, 200, 500, 800, 1000, 1200, 1500, 2000, 2500, 3000, 3500, 4000, 4500, 5000, etc. The number average molecular weight of the polyoxypropylene triol is preferably 250-6000, such as 250, 500, 1000, 1500, 2000, 2500, 3000, 3500, 4000, 4500, 5000, 5500, 6000, etc. The number average molecular weight of the polytetrahydrofuran diol is preferably 500-4000, such as 500, 800, 1000, 1200, 1500, 2000, 2500, 3000, 3500, 4000, etc. The number average molecular weight of the bisphenol A modified polyether polyol is preferably 500-4000, such as 500, 800, 1000, 1200, 1500, 2000, 2500, 3000, 3500, 4000, etc. The number average molecular weight of the polyoxyethylene polyol is 500-4000, such as 500, 800, 1000, 1200, 1500, 2000, 2500, 3000, 3500, 4000, etc.
[0039] In the present invention, the number average molecular weight of the castor oil polyol I and the castor oil polyol II is preferably independently 400-5000, such as 400, 800, 1000, 1200, 1500, 1800, 2000, 2200, 2500, 2800, 3000, 3200, 3500, 3800, 4000, 4200, 4500, 4800, 5000 or any value therebetween; the functionality is preferably independently 2-4, such as 2, 3 or 4. The castor oil polyol I and the castor oil polyol II can be independently selected from unmodified castor oil polyol and / or modified castor oil polyol.
[0040] In the present invention, the polyisocyanate I and polyisocyanate II are compounds with two or more isocyanate groups at the molecular chain terminals, specifically aromatic isocyanates and / or aliphatic isocyanates, preferably independently selected from a mixture of diphenylmethane-4,4'-diisocyanate and diphenylmethane-2,2'-diisocyanate and / or diphenylmethane-2,4'-diisocyanate, carbodiimide-modified MDI, polyether-modified MDI, polymethylene polyphenyl polyisocyanate, 4,4'-dicycloethylmethane diisocyanate and isophorone diisocyanate, more preferably a mixture of diphenylmethane-4,4'-diisocyanate and diphenylmethane-2,2'-diisocyanate and / or diphenylmethane-2,4'-diisocyanate. When the polyisocyanate I and the polyisocyanate II are a mixture of diphenylmethane-4,4'-diisocyanate and diphenylmethane-2,2'-diisocyanate and / or diphenylmethane-2,4'-diisocyanate, it is more conducive to reducing the low-temperature modulus.
[0041] In the present invention, the filler I and filler II are preferably each independently selected from at least one of aluminum hydroxide, aluminum oxide, calcium carbonate, talcum powder, quartz powder, mica powder, titanium dioxide, white carbon black, bentonite and carbon black.
[0042] In the present invention, the molecular sieve I and molecular sieve II are preferably independently selected from at least one of mordenite, Y zeolite, ZSM-5 molecular sieve, MCM-22 molecular sieve, MCM-56 molecular sieve and Beta molecular sieve.
[0043] In the present invention, specific examples of the auxiliary agent I include, but are not limited to: at least one of color paste, defoamer, dewatering agent, rheological agent, leveling agent, wetting agent, coupling agent, stabilizer and catalyst. Specific examples of the auxiliary agent II include, but are not limited to: at least one of defoamer, stabilizer, polymerization inhibitor, leveling agent, leveling agent and thixotropic agent.
[0044] In the present invention, the terms "Ⅰ" and "Ⅱ" are only used to distinguish the same type of substances introduced from different raw material ends for the convenience of description and have no other special meanings.
[0045] The preparation method of the two-component polyurethane structural adhesive provided by the present invention comprises the following steps:
[0046] Preparation of component A: Mix all the raw materials in component A evenly and then remove the vacuum to obtain component A;
[0047] Preparation of component B: Mix the raw materials in component B evenly and then de-vacuum to obtain component B.
[0048] In addition, the present invention also provides the use of the above-mentioned two-component polyurethane structural adhesive in the fixation of glass on frameless windows of new energy vehicles and structural bonding at low temperatures.
[0049] The present invention will be described in detail below through examples.
[0050] The raw materials and sources involved in the preparation examples and embodiments are as follows: dimer acid polyester polyol, purchased from Croda Corporation, brand Priplast 1838, Mn is 2000 g / mol; polycaprolactone polyol, purchased from Daicel Corporation of Japan, brand PLACCEL220EB, Mn is 2000 g / mol, functionality is 2; polycarbonate polyol, purchased from Asahi Kasei Corporation of Japan, brand T5652, Mn is 2000 g / mol, functionality is 2; polyoxypropylene glycol purchased from Jiangsu Zhongshan Chemical Co., Ltd., brand N-220, Mn is 2000 g / mol, functionality is 2; polytetrahydrofuran diol , purchased from BASF, Germany, brand THF-20P, Mn is 2000g / mol, functionality is 2; bisphenol A polyoxyethylene ether, purchased from SEPPIC, France, brand HP2002, Mn is 2000g / mol, functionality is 2; unmodified castor oil polyol, purchased from Nanjing Xinxu Industry and Trade Co., Ltd., brand Castoroil, Mn is 2000g / mol, functionality is 2.7; modified castor oil polyol, purchased from Ito, Japan, brand URIC AC009, Mn is 2000g / mol, functionality is 2.5; fumed silica was purchased from Cabot, brand TS-610; the additives are all defoaming additives, purchased from BYK, brand BYK-A 506.
[0051] Preparation Example 1 Preparation of polyurethane prepolymer
[0052] 100g of dimer acid polyester polyol, 100g of polycaprolactone polyol, 100g of polyoxypropylene glycol and 100g of unmodified castor oil polyol were vacuum dehydrated at 100°C to a water content of less than 300ppm, and then the system temperature was reduced to 50°C, and 200g of diphenylmethane-4,4'-diisocyanate, 200g of diphenylmethane-2,2'-diisocyanate and 200g of diphenylmethane-2,4'-diisocyanate were added, and under nitrogen protection, the temperature was raised to 78°C±0.5°C while stirring to react until the NCO content reached 23wt%, and the polyurethane prepolymer was obtained after cooling, which was recorded as JU-100.
[0053] Preparation Example 2 Preparation of polyurethane prepolymer
[0054] 100g of dimer acid polyester polyol, 200g of polycarbonate polyol, 200g of polytetramethylene glycol, and 200g of unmodified castor oil polyol were vacuum dehydrated at 120°C to a water content of less than 300ppm, and then the system temperature was reduced to 45°C, and 100g of diphenylmethane-4,4'-diisocyanate, 100g of diphenylmethane-2,2'-diisocyanate and 100g of diphenylmethane-2,4'-diisocyanate were added. Under nitrogen protection, the temperature was raised to 82°C±0.5°C while stirring to react until the NCO content reached 5wt%. After cooling, a polyurethane prepolymer was obtained, which was recorded as JU-200.
[0055] Preparation Example 3 Preparation of polyurethane prepolymer
[0056] 100g of dimer acid polyester polyol, 100g of polycaprolactone polyol, 150g of polycarbonate polyol, 100g of polyoxypropylene glycol, 50g of bisphenol A polyoxyethylene ether, and 100g of modified castor oil polyol were vacuum dehydrated at 110°C to a water content of less than 300ppm, and then the system temperature was reduced to 55°C, and 200g of diphenylmethane-4,4'-diisocyanate, 100g of diphenylmethane-2,2'-diisocyanate and 100g of diphenylmethane-2,4'-diisocyanate were added, and under nitrogen protection, the temperature was raised to 80°C±0.5°C while stirring to react until the NCO content reached 10wt%, and the polyurethane prepolymer was obtained after cooling, which was recorded as JU-300.
[0057] Preparation Example 4 Preparation of polyurethane prepolymer
[0058] A polyurethane prepolymer was prepared according to the method of Preparation Example 1, except that polyoxypropylene glycol and unmodified castor oil polyol were replaced by polycaprolactone polyol in equal parts by weight. The remaining conditions were the same as those of Preparation Example 1 to obtain a polyurethane prepolymer, which was recorded as JU-400.
[0059] Preparation Example 5 Preparation of polyurethane prepolymer
[0060] A polyurethane prepolymer was prepared according to the method of Preparation Example 1, except that diphenylmethane-2,2'-diisocyanate and diphenylmethane-2,4'-diisocyanate were both replaced by diphenylmethane-4,4'-diisocyanate in equal parts by weight. The remaining conditions were the same as those of Preparation Example 1 to obtain a polyurethane prepolymer, which was recorded as JU-500.
[0061] Comparative Preparation Example 1 Preparation of Reference Polyurethane Prepolymer
[0062] A polyurethane prepolymer was prepared according to the method of Preparation Example 1, except that the polycaprolactone polyol, polyoxypropylene glycol and unmodified castor oil polyol were all replaced by 1,3-propylene glycol in equal parts by weight, and the other conditions were the same as those of Preparation Example 1 to obtain a reference polyurethane prepolymer, which was recorded as DJU-600.
[0063] Comparative Preparation Example 2 Preparation of Reference Polyurethane Prepolymer
[0064] A polyurethane prepolymer was prepared according to the method of Preparation Example 1, except that the dimer acid polyester polyol (Priplast 1838 from Croda Corporation) was replaced by the same weight portion of non-dimer acid polyester polyol (BASF THF-20P). The other conditions were the same as those in Preparation Example 1 to obtain a reference polyurethane prepolymer, which was recorded as DJU-700.
[0065] Example 1 Preparation of two-component polyurethane structural adhesive
[0066] Component A: 10 g of polycaprolactone polyol, 300 g of polyoxypropylene glycol, 300 g of unmodified castor oil polyol, 50 g of plasticizer (di-n-butyl phthalate) and 10 g of auxiliary agent were mixed for 30 min, and then 310 g of filler, 10 g of molecular sieve (ZSM-5 molecular sieve) and 10 g of fumed silica were added and mixed for 60 min, and the component A was obtained after de-vacuuming;
[0067] Component B: 150 g of diphenylmethane-4,4'-diisocyanate, 350 g of polyurethane prepolymer JU-100, 50 g of plasticizer (di-n-butyl phthalate), and 10 g of additive were mixed for 30 min, and then 420 g of filler, 10 g of molecular sieve (ZSM-5 molecular sieve) and 10 g of fumed silica were added and mixed for 60 min, and the component B was obtained after de-vacuuming;
[0068] Component A and component B are mixed evenly in a volume ratio of 1:1 (the molar ratio of hydroxyl groups in polyester polyol, polyether polyol and castor oil polyol to isocyanate groups in isocyanate and polyurethane prepolymer is 1:1.250) to obtain a two-component polyurethane structural adhesive.
[0069] Example 2 Preparation of two-component polyurethane structural adhesive
[0070] Component A: 900 g of polycaprolactone polyol, 10 g of polyoxypropylene glycol, 10 g of unmodified castor oil polyol, 10 g of plasticizer (dioctyl phthalate) and 10 g of auxiliary agent were mixed for 30 min, and then 40 g of filler, 10 g of molecular sieve (ZSM-5 molecular sieve) and 10 g of fumed silica were added and mixed for 60 min, and the component A was obtained after de-vacuuming;
[0071] Component B: 150 g of diphenylmethane-4,4'-diisocyanate, 550 g of polyurethane prepolymer JU-200, 50 g of plasticizer (dioctyl phthalate), and 10 g of additive were mixed for 30 min, and then 220 g of filler, 10 g of molecular sieve (ZSM-5 molecular sieve) and 10 g of fumed silica were added and mixed for 60 min, and the component B was obtained after de-vacuuming;
[0072] Component A and component B are mixed evenly in a volume ratio of 1:1 (the molar ratio of hydroxyl groups in polyester polyol, polyether polyol and castor oil polyol to isocyanate groups in isocyanate and polyurethane prepolymer is 1:1) to obtain a two-component polyurethane structural adhesive.
[0073] Example 3 Preparation of two-component polyurethane structural adhesive
[0074] Component A: 450 g of polycaprolactone polyol, 150 g of polyoxypropylene glycol, 150 g of unmodified castor oil polyol, 50 g of plasticizer (di-n-butyl phthalate) and 10 g of auxiliary agent were mixed for 30 min, and then 170 g of filler, 10 g of molecular sieve (ZSM-5 molecular sieve) and 10 g of fumed silica were added and mixed for 60 min, and the component A was obtained after de-vacuuming;
[0075] Component B: 150 g of diphenylmethane-4,4'-diisocyanate, 450 g of polyurethane prepolymer JU-300, 50 g of plasticizer (di-n-butyl phthalate), and 10 g of additive were mixed for 30 min, and then 320 g of filler, 10 g of molecular sieve (ZSM-5 molecular sieve) and 10 g of fumed silica were added and mixed for 60 min, and the component B was obtained after de-vacuuming;
[0076] Component A and component B are mixed evenly in a volume ratio of 1:1 (the molar ratio of hydroxyl groups in polyester polyol, polyether polyol and castor oil polyol to isocyanate groups in isocyanate and polyurethane prepolymer is 1:1.1) to obtain a two-component polyurethane structural adhesive.
[0077] Example 4 Preparation of two-component polyurethane structural adhesive
[0078] A two-component polyurethane structural adhesive was prepared according to the method of Example 1, except that the polyurethane prepolymer JU-100 was replaced by the same weight portion of the polyurethane prepolymer JU-400, and the other conditions were the same as in Example 1 to obtain a two-component polyurethane structural adhesive.
[0079] Example 5 Preparation of two-component polyurethane structural adhesive
[0080] A two-component polyurethane structural adhesive was prepared according to the method of Example 1, except that the polyurethane prepolymer JU-100 was replaced by the same weight portion of the polyurethane prepolymer JU-500, and the other conditions were the same as in Example 1 to obtain a two-component polyurethane structural adhesive.
[0081] Comparative Example 1 Preparation of a Reference Two-Component Polyurethane Structural Adhesive
[0082] A two-component polyurethane structural adhesive was prepared according to the method of Example 4, except that the polyurethane prepolymer JU-100 was replaced by the reference polyurethane prepolymer DJU-600 in the same weight portion, and the other conditions were the same as in Example 4 to obtain a reference two-component polyurethane structural adhesive.
[0083] Comparative Example 2 Preparation of Reference Two-Component Polyurethane Structural Adhesive
[0084] A two-component polyurethane structural adhesive was prepared according to the method of Example 4, except that the polyurethane prepolymer JU-100 was replaced by the reference polyurethane prepolymer DJU-700 in the same weight portion, and the other conditions were the same as in Example 4 to obtain a reference two-component polyurethane structural adhesive.
[0085] Test Case
[0086] (1) DMA room temperature (25°C) modulus: The sample size is 50 mm*7 mm*0.3 mm. The film stretching method is adopted. The temperature is increased from -40°C to 90°C at a test frequency of 1 Hz and a heating rate of 2°C / min. The DMA curve is obtained and the modulus at 25°C is marked, that is, the room temperature modulus. The results are shown in Table 1.
[0087] (2) DMA low temperature (-40°C) modulus: The specimen size is 50 mm*7 mm*0.3 mm. The film stretching method is adopted. The temperature is increased from -40°C to 90°C at a test frequency of 1 Hz and a heating rate of 2°C / min. The DMA curve is obtained and the modulus at -40°C, i.e., the low temperature modulus, is marked. The results are shown in Table 1.
[0088] (3) Initial bonding strength: The two-component polyurethane structural adhesive obtained in the above examples and comparative examples was coated on 6061 aluminum sheets respectively, overlapped and pressed with glass sheets to make test samples, with a bonding area of 12.5.0 mm × 25.0 mm, and the thickness of the adhesive layer was ensured to be 0.15 mm. After curing at 80°C for 5 min and cooling at room temperature for 3 min, the two sheets were pulled apart in opposite directions using a universal testing machine. The measured force value was recorded as strength (MPa), which is the initial bonding strength of the just-made sample. The results are shown in Table 1.
[0089] (4) Resistance to wet and hot aging: The two-component polyurethane structural adhesive obtained in the above embodiments and comparative examples was coated on 6061 aluminum sheets respectively, overlapped and pressed with glass sheets to make test samples, with a bonding area of 12.5.0 mm × 25.0 mm, and the thickness of the adhesive layer was ensured to be 0.15 mm. After curing at room temperature (25°C) for 7 days, it was placed at a temperature of 85°C and a humidity of 85% RH for 1000 hours, and then the bonding strength was tested using a universal testing machine. The bonding strength value is the bonding strength after wet and hot aging resistance. The higher the wet and hot aging resistance, the better the wet and hot aging resistance, and vice versa. The obtained results are shown in Table 1.
[0090] (5) Thermal shock resistance: Aluminum 6061-glue-glass structure was prepared, in which the radius of the glue after pressing was 8-9 mm and the thickness was 1.2 mm. After being completely cured, it was placed in a high and low temperature test chamber for testing. The sample was placed in an environment of -40℃±1℃ for 2 hours and then quickly transferred to an environment of 85℃±1℃ for 2 hours. The temperature conversion was completed within 2 minutes, which was 1 cycle. After reaching the specified number of cycles, the sample was taken out to observe whether there was debonding and whether the glass was broken. The results are shown in Table 1.
[0091] Table 1
[0092]
[0093] It can be seen from the results in Table 1 that the two-component polyurethane structural adhesive provided by the present invention has the characteristics of low-temperature low modulus, excellent resistance to moisture and heat aging and resistance to cold and hot shock, etc. Specifically, the low-temperature DMA modulus at -40°C can be reduced to below 1100MPa, the DMA modulus at room temperature can be reduced to below 500MPa, the initial strength can reach above 0.81MPa, the bonding strength after double 85 aging for 1000h is above 5MPa, and there is no debonding and glass cracking after 300 cold and hot cycles.
[0094] From the comparison between Example 1 and Example 4, it can be seen that compared with the use of a single polyol, when the polyol mixture contains polyester polyol II, polyether polyol II and castor oil polyol II at the same time, it is more conducive to the improvement of initial strength and heat and humidity aging resistance.
[0095] From the comparison between Example 1 and Example 5, it can be seen that compared with the use of a single polyisocyanate, when the polyisocyanate I and the polyisocyanate II are a mixture of diphenylmethane-4,4'-diisocyanate and diphenylmethane-2,2'-diisocyanate and / or diphenylmethane-2,4'-diisocyanate, the low-temperature modulus can be further reduced while ensuring that the initial strength and heat and humidity aging resistance are equivalent.
[0096] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention without departing from the principles and intent of the present invention.
Claims
1. A two-component polyurethane structural adhesive, characterized in that: The two-component polyurethane structural adhesive contains component A and component B in a volume ratio of 1:(0.25-4); the component A contains polyester polyol I, polyether polyol I, castor oil polyol I and plasticizer I in a mass ratio of 100:(1-9000):(1-9000):(1-3000); the component B contains polyisocyanate I, polyurethane prepolymer and plasticizer II in a mass ratio of 100:(50-8500):(10-3000); The polyurethane prepolymer is obtained by reacting a polyol mixture with polyisocyanate II, wherein the polyol mixture contains dimer acid polyester polyol and other polyols, wherein the other polyols are selected from at least one of polyester polyol II, polyether polyol II and castor oil polyol II other than dimer acid polyester polyol; the NCO content of the polyurethane prepolymer is 5-23wt%; The plasticizer I and the plasticizer II are each independently selected from at least one of phthalic acid esters, aliphatic diacid esters, benzoic acid glycol esters and phosphate ester plasticizers.
2. The two-component polyurethane structural adhesive according to claim 1, characterized in that: The A component contains the following raw materials in the A component in percentage by mass: The B component contains the following raw materials in the B component in percentage by mass:
3. The two-component polyurethane structural adhesive according to claim 1, characterized in that: The polyurethane prepolymer is prepared according to the following method: vacuum dehydrating a polyol mixture at 100-120° C. until the water content is less than 300 ppm, lowering the temperature of the dehydrated polyol mixture to 45-55° C., adding polyisocyanate II, and reacting at 78-82° C. while stirring under inert gas protection until the NCO content reaches 5-23wt%, and then cooling to obtain a polyurethane prepolymer; Preferably, the mass ratio of dimer acid polyester polyol to other polyols in the polyol mixture is (0.1-10):1; Preferably, the dimer acid structural unit in the dimer acid polyester polyol is selected from at least one of a polyoleic acid structural unit, a polylinoleic acid structural unit, a polylinolenic acid structural unit and a polyarachidonic acid structural unit; Preferably, the number average molecular weight of the dimer acid polyester polyol is 1000-3000.
4. The two-component polyurethane structural adhesive according to claim 1, characterized in that: The molar ratio of the total content of hydroxyl groups to the total content of isocyanate groups in the two-component polyurethane structural adhesive is 1:(1-1.5).
5. The two-component polyurethane structural adhesive according to claim 1, characterized in that: The number average molecular weights of the polyester polyol I and the polyester polyol II in the component A are independently 500-4000, and the functionality is independently 2-4.
6. The two-component polyurethane structural adhesive according to claim 1, characterized in that: The polyether polyol I and polyether polyol II are independently selected from at least one of polyoxypropylene diol with a number average molecular weight of 100-5000, polyoxypropylene triol with a number average molecular weight of 250-6000, polytetrahydrofuran diol with a number average molecular weight of 500-4000, bisphenol A modified polyether polyol with a number average molecular weight of 500-4000 and polyoxyethylene polyol with a number average molecular weight of 500-4000.
7. The two-component polyurethane structural adhesive according to claim 1, characterized in that: The number average molecular weight of the castor oil polyol I and the castor oil polyol II are independently 400-5000, and the functionality is independently 2-4.
8. The two-component polyurethane structural adhesive according to claim 1, characterized in that: The polyisocyanate I and polyisocyanate II are independently selected from at least one of a mixture of diphenylmethane-4,4'-diisocyanate and diphenylmethane-2,2'-diisocyanate and / or diphenylmethane-2,4'-diisocyanate, carbodiimide-modified MDI, polyether-modified MDI, polymethylene polyphenyl polyisocyanate, 4,4'-dicycloethylmethane diisocyanate and isophorone diisocyanate.
9. The two-component polyurethane structural adhesive according to claim 2, characterized in that: The filler I and filler II are each independently selected from at least one of aluminum hydroxide, aluminum oxide, calcium carbonate, talcum powder, quartz powder, mica powder, titanium dioxide, white carbon black, bentonite and carbon black; The molecular sieve I and molecular sieve II are each independently selected from at least one of mordenite, Y zeolite, ZSM-5 molecular sieve, MCM-22 molecular sieve, MCM-56 molecular sieve and Beta molecular sieve; The auxiliary agent I is selected from at least one of a color paste, a defoamer, a dewatering agent, a rheological agent, a leveling agent, a wetting agent, a coupling agent, a stabilizer and a catalyst; The auxiliary agent II is selected from at least one of a defoamer, a stabilizer, an inhibitor, a leveling agent, a leveling agent and a thixotropic agent.
10. The method for preparing the two-component polyurethane structural adhesive according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: Preparation of component A: Mix all the raw materials in component A evenly and then remove the vacuum to obtain component A; Preparation of component B: Mix the raw materials in component B evenly and then de-vacuum to obtain component B.
11. Application of the two-component polyurethane structural adhesive according to any one of claims 1 to 9 in fixing glass on frameless windows of new energy vehicles and structural bonding at low temperatures.