High-strength non-oriented electrical steel with excellent magnetic performance and manufacturing method thereof
By optimizing the chemical composition and process flow of Si, Al, Mn, P, Ce, it solves the problem of magnetic performance degradation when the strength is improved, and achieves high-strength without iron loss, high strength and excellent magnetic performance Oriented to electrical steel to meet the needs of new energy vehicle drive motors.
Patent Information
- Application Number
- CN202410909222.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-07-08
AI Technical Summary
The existing non-oriented electrical steels are difficult to meet the requirements of new energy vehicle drive motors for low iron loss and high magnetic induction while increasing their strength. Traditional strengthening methods such as precipitation strengthening and solid solution strengthening will lead to abnormal grain growth or magnetic properties. decline.
By optimizing the chemical composition of Si, Al, Mn, P and Ce, combining smelting, continuous casting, hot rolling, curling, regularization, cold rolling and annealing processes, the C content is controlled at 0.001-0.005% and Si is 1.1-2.0% , Mn is between 0.4-0.7%, Al is between 1.1-2.0%, P is between 0.2-0.35%, and Ce is between 0.015-0.035%, so as to achieve the goals of low iron loss, high strength and excellent magnetic properties.
It is realized without adding high-temperature annealing and high-valent alloy elements to obtain high-strength non-oriented electrical steel with low iron loss, low hysteresis loss, high yield strength and tensile strength. The magnetic induction strength B50 is between 1.68-1.75T, iron is The loss P1.0/400 is between 15.5-19.5W/Kg, the yield strength Rel is between 550-650MPa, and the tensile strength Rm is between 650-750MPa.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metallurgical materials, and in particular to a high-strength non-oriented electrical steel with excellent magnetic properties and a manufacturing method thereof. Background Art
[0002] With the increasing requirements for environmental protection, new energy vehicles, as an environmentally friendly means of transportation, are developing more and more rapidly; the drive motor is one of the core components of new energy vehicles and needs to meet the requirements of miniaturization, high efficiency and high torque. The miniaturization and high efficiency of the motor require that the non-oriented electrical steel used to make its core should have low iron loss and high magnetic induction; when the speed increases, the huge centrifugal force generated can easily damage the motor rotor, so the non-oriented electrical steel needs to have high strength to ensure safety at high speeds. Traditional non-oriented silicon steel can meet the requirements of low iron loss and high magnetic induction, but the strength is low. Strength and iron loss are contradictory indicators. The increase in strength will reduce the magnetic properties. Therefore, it is an important research task to develop low iron loss and high strength non-oriented electrical steel for new energy vehicle drive motors.
[0003] The main methods to improve the strength of non-oriented electrical steel include precipitation strengthening, solid solution strengthening, dislocation strengthening and composite strengthening. Precipitation strengthening mainly improves the strength by forming fine carbide particles through microalloy elements and C. These fine carbide particles will hinder the rotation of magnetic domains and reduce magnetic properties. Solid solution strengthening improves the strength through elements such as Si, Mn, Al, and Cu, but too high Si can easily lead to difficulties in cold rolling. The addition of Cu will cause "copper brittleness", which increases the difficulty of rolling. High-temperature annealing is required to temporarily dissolve Cu and delay recrystallization. Higher heating temperatures will cause abnormal grain growth, which is not conducive to improving strength.
[0004] Japan has been researching high-strength non-oriented electrical steel since the 1980s. For example, Nippon Steel & Sumitomo Metal Corporation (formerly Nippon Steel & Sumitomo Metal, referred to as NSSMC) and JFE, patent 201280004130.1 discloses a high-strength non-oriented electrical steel sheet, which is added with 0.5-3.0% Ni and 0.5-3.0% Cu, and annealed at high temperature to make the interaction between Cu precipitates and sulfides, so as to obtain good magnetic properties and excellent strength properties. 1.0 / 400 =20.2-30.5W / kg, yield strength R el Japanese patent 200980113090.2 discloses a high-strength non-oriented electrical steel sheet and its manufacturing method, by adding 0.5-3.0% Cu, Cu precipitates and strengthens the steel sheet after a high-temperature annealing process at 950-1000°C, but the annealing temperature is high, and some grains grow abnormally, which is not conducive to the iron loss P 1.0 / 400 The reduction and magnetic induction B 50 The improvement of magnetic induction B 501.60-1.65T, iron loss P 1.0 / 400 It is 25.0-30.0W / kg, and the iron loss and magnetic induction do not meet the high efficiency requirements of non-oriented electrical steel for new energy vehicles.
[0005] China is also accelerating the pace of research and development of high-strength non-oriented electrical steel. For example, Chinese patent CN106282781A discloses a method for preparing high-strength non-oriented silicon steel based on nano-Cu precipitation strengthening. The nano-Cu precipitation has little hindering effect on the movement of magnetic domain walls, and has almost no effect on the magnetic induction while greatly improving the strength. However, the method of strengthening by Cu precipitation requires high-temperature annealing to temporarily dissolve Cu, delay recrystallization, and control the recrystallization rate. However, high-temperature annealing causes some grains to grow abnormally, and the magnetic induction B 50 1.67-1.74T, iron loss P 1.0 / 400 It is 22.5-31.5W / kg, and the iron loss is relatively high.
[0006] Chinese patents CN106435358A and CN105803311A use twin-roller thin strip continuous casting technology, add precipitation strengthening element Nb, and combine composition design, rolling and heat treatment to produce non-oriented electrical steel with excellent magnetic properties and high strength. 50 1.68-1.73T, iron loss P 1.0 / 400 It is 25.5-37.5W / kg, and the iron loss is relatively high.
[0007] Baosteel patent CN108286014A improves strength through Si solid solution strengthening ability, but the high Si content reduces the toughness of the steel plate, which is not conducive to product processing; China patent CN106435358A adopts ultra-low C steelmaking technology and improves strength by adding precipitation strengthening element Nb, but its finished product iron loss P 1.0 / 400 The highest is 28.0-38.2W / kg; Chinese patent CN111235461A adopts a high C (0.03-0.08%) component system to improve the strength of non-oriented silicon steel by adding Nb, Ti and trace rare earth, but C and Ti will reduce the magnetic properties of non-oriented silicon steel.
[0008] Ma Steel's patent CN113981329A uses a compounding method of Ce+Sn, which helps to improve the strength and magnetic properties of non-oriented electrical steel. However, when adjusting the ratio of the two, it is necessary to take into account the negative effects of the two components Ce and Sn at the same time, which is bound to affect the effect of the separate regulation and improvement of the strength and magnetic properties of non-oriented electrical steel, and cannot achieve the expected effect. In addition, the cost of using Sn is relatively higher than that of Ce. In addition, the Si content of 2.4-3.0% used in this patent is still relatively high, which will affect the magnetic properties and toughness of electrical steel. Summary of the invention
[0009] In view of the above problems, the present invention proposes a high-strength non-oriented electrical steel with excellent magnetic properties and a manufacturing method thereof, so that the electrical steel has lower iron loss and higher strength. The present invention optimizes the content of Si, Al, Mn, P, and Ce, removes harmful impurities, and improves the strength through precipitation strengthening, and then performs smelting, continuous casting, hot rolling, normalizing, cold rolling, and annealing to finally obtain high-strength non-oriented silicon steel with excellent magnetic properties.
[0010] In order to solve the above technical problems, the present invention is implemented by the following technical solutions:
[0011] The present invention provides a high-strength non-oriented electrical steel with excellent magnetic properties. The chemical composition of the non-oriented electrical steel is as follows by weight percentage: C: 0.001-0.005%, Si: 1.1-2.0%, Mn: 0.4-0.7%, Al: 1.1-2.0%, P: 0.2-0.35%, S: ≤0.005%, Ce: 0.015-0.035%, and the balance is iron and inevitable impurities.
[0012] Preferably, the chemical composition of the non-oriented electrical steel is as follows by weight: C: 0.002%, Si: 1.95%, Mn: 0.69%, Al: 2.0%, P: 0.34%, S: 0.001%, Ce: 0.025%, and the remainder is iron and unavoidable impurities.
[0013] Preferably, the weight ratio Mn / P≧2.
[0014] Preferably, the weight percentage content of Si is less than Al.
[0015] Preferably, the magnetic properties of the non-oriented electrical steel are: when the thickness is 0.30 mm, B 50 =1.68-1.75T, P 1.0 / 400 =15.5-19.5W / Kg, yield strength Rel is 550-650MPa, tensile strength Rm is 650-750MPa, elongation A 50 ≤20%.
[0016] The present invention also provides a method for manufacturing high-strength non-oriented electrical steel with excellent magnetic properties, comprising the following steps: molten iron pretreatment → converter smelting → continuous casting → hot rolling → curling → normalizing → cold rolling → annealing → finished product.
[0017] Preferably, the hot rolling start temperature is 1100-1200° C., and the hot rolling finish temperature is 900-950° C., which can further reduce the risk of phosphorus embrittlement.
[0018] Preferably, the curling temperature is 680-710°C.
[0019] Preferably, the normalizing temperature is 900-1000°C.
[0020] Preferably, the annealing temperature is 850-950°C.
[0021] The chemical composition design of the present invention controls the content of the main alloy elements as follows:
[0022] C: The present invention controls the C content mainly to prevent C from deteriorating the magnetic properties. The present invention limits the C content to 0.001-0.005%.
[0023] Si: As the Si content increases, the strength of the steel plate increases, the magnetic induction decreases, and the brittleness of the steel plate increases, which is not conducive to the surface quality control of the hot-rolled coil. Therefore, the Si content in the steel should be reduced in the present invention. The Si content in the present invention is 1.1-2.0%.
[0024] Mn: Mn is beneficial to improve the resistivity of electrical steel and reduce iron loss. It can also improve strength through solid solution strengthening. Therefore, the Mn content in the present invention is set to 0.4-0.7%.
[0025] Al: As Al content increases, steel plate strength increases and magnetic induction increases, but too high Al content can easily cause molten steel to become sticky, so the present invention controls the Al content to be 1.1-2.0%. Al content can reduce iron loss without reducing magnetic induction, and Al can also improve steel plate plasticity and reduce the impact of phosphorus embrittlement on steel plates. At the same time, Al combines with N to form AlN, which can refine grains and improve strength, so the weight percentage content of Si and Al is set to Si%<Al%.
[0026] P: P will produce segregation, refine grains, increase strength, and improve texture, but Fe3P segregation will make the steel plate brittle and reduce toughness, so the present invention controls 0.2-0.35%. If the P content is too high, the steel plate is prone to phosphorus embrittlement. Adding Mn can improve the toughness and plasticity of the steel plate and reduce the influence of phosphorus embrittlement on the steel plate, so the weight percentage content Mn / P ≥ 2.
[0027] S: S and Mn in steel can form plastic MnS inclusions to reduce hot brittleness, but will cause the strip steel to form a banded structure, reduce the toughness and formability of the steel plate, and S has a great influence on the magnetic properties. The present invention controls the S content to ≤0.005%.
[0028] Ce: Ce is easy to form Ce oxysulfide with impurity elements such as O and S in steel during steelmaking, which has the effect of purifying steel and is beneficial to improving magnetic properties. The remaining Ce after steelmaking will precipitate, hindering grain growth, making grains finer, and improving steel plate strength. However, grain refinement will lead to increased hysteresis loss, so the weight percentage of Ce is 0.015-0.035%.
[0029] The manufacturing method of the high-strength non-oriented electrical steel with excellent magnetic properties requires the following steps: molten iron pretreatment → converter smelting → continuous casting → hot rolling → curling → normalizing → cold rolling → annealing → finished product.
[0030] (1) Hot metal pretreatment: In the hot metal pretreatment process, taking pre-slag and post-slag removal measures to adjust the [S] element can reduce harmful elements in the molten steel. Adding self-circulating scrap steel in the early and middle stages of decarburization to modify the ladle top slag can help reduce impurity elements in the molten steel.
[0031] (2) Hot rolling: The starting temperature of hot rolling is 1100-1200℃, and the final temperature of hot rolling is 900-950℃. The hot rolling temperature should not be too high. Too high temperature will lead to the refinement of inclusions and deteriorate the magnetic properties.
[0032] (3) Coiling: The coiling temperature is 680-710℃. The coiling temperature helps to improve the grain uniformity of the product and improve the magnetic induction.
[0033] (3) Normalizing: The normalizing temperature is 900-1000℃. If the normalizing temperature is too high, the grains will grow abnormally, the plasticity will decrease, and cold rolling will be difficult.
[0034] (4) Annealing: The annealing temperature is 850-950℃. It is the last process to adjust the magnetic properties. The appropriate annealing temperature helps to balance the iron loss and magnetic induction indicators.
[0035] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0036] The role and combined role of the important components of the present invention: (1) The present invention simplifies the original Sn+Ce compounding method into a method of adding Ce alone by optimizing and adjusting the chemical composition. The addition of Ce alone not only retains the effect of the original Sn+Ce, but also eliminates the relatively high cost of Sn. When improving the strength and magnetic properties of non-oriented silicon steel, it is only necessary to overcome the negative impact of the Ce dosage. The strength and magnetic properties of electrical steel performance can be more accurately controlled by adjusting the Ce dosage alone, and the operation is simple. (2) Microalloying effect of Ce: The addition of Ce plays a dual role. One is to purify the steel and improve the magnetic properties. The other is to precipitate through the microalloying process, hinder the growth of grains, further refine the grains and improve the strength. Although grain refinement may increase hysteresis loss, this negative impact is minimized by reasonably controlling the Ce content at 0.015-0.035%. (3) Balance between Si and Al: This application further reduces the Si content to 1.1%-2.0%. Si is a key element that affects the magnetic properties and strength of electrical steel. A lower Si content can improve the magnetic permeability of the material to a certain extent, which is conducive to obtaining better magnetic properties, but also affects the mechanical strength of the material. Al can improve strength and magnetic induction while improving strength by forming AlN with nitrogen to refine the grains, making up for the defect of insufficient strength caused by the reduction of Si content, enhancing the plasticity of the material and reducing the impact of phosphorus embrittlement. By setting Si<Al, an optimal balance between strength, magnetism and plasticity is achieved. (4) Strengthening effect of Mn: Mn not only improves the resistivity of the material and reduces iron loss, but also enhances strength through solid solution strengthening. At the same time, the addition of Mn helps to alleviate the brittleness problem caused by P. Ensuring a weight ratio of Mn / P≥2 is the key to reducing the impact of phosphorus embrittlement. (5) Fine control of P: An appropriate amount of P can refine the grains and improve strength, but an excessive amount will lead to brittleness. By limiting the P content to 0.2-0.35% and operating in a high Mn environment, the needs of strength improvement and toughness are effectively balanced.
[0037] The synergistic effects of the process of the present invention are as follows: (1) Pretreatment and converter smelting: The use of slag removal in the early and late stages and self-circulating scrap steel effectively reduces impurity elements, provides a pure raw material basis for subsequent processes, and is a prerequisite for the formation of high-quality products. (2) Temperature control of the hot rolling process: By setting the hot rolling start temperature at 1100-1200°C and the final rolling temperature at 900-950°C, it not only ensures the good plastic processing properties of the material, but also avoids the refinement of inclusions at high temperatures, thereby protecting the magnetic properties from damage. (3) Precise adjustment of the curling and normalizing temperatures: The curling temperature is set at 680-710°C, which helps to uniformly distribute the grains; the normalizing temperature of 900-1000°C ensures the stability of the grains and provides a good organizational basis for subsequent cold rolling, all of which have a direct impact on the mechanical properties and magnetic properties of the final product. (4) Careful arrangement of annealing process: The annealing temperature of 850-950℃ is the last step in adjusting the magnetic properties. By selecting this temperature range, the relationship between iron loss and magnetic induction is balanced, ensuring the high performance of the material in practical applications.
[0038] In summary, the present invention achieves a dual improvement in the magnetic properties and mechanical properties of high-strength non-oriented electrical steel through carefully designed chemical composition and optimized manufacturing process, especially without relying on high-valent alloying elements (such as Sn, Cr, Cu, Ti), through the effective combination of Si, Al, Mn, P, Ce and the regulation of key process parameters, showing significant innovation and practicality. DETAILED DESCRIPTION
[0039] In order to enable those skilled in the art to better understand the technical solution of the present invention, the preferred implementation scheme of the present invention is described below in conjunction with specific embodiments, but it should not be understood as limiting the present invention and is only used as an example.
[0040] The experimental methods or test methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials are obtained from conventional commercial channels or prepared by conventional methods unless otherwise specified.
[0041] The present invention is further described in detail below in conjunction with specific embodiments.
[0042] The inventors utilize the optimized contents of Si, Al, Mn, P and Ce and the characteristics of Ce oxysulfide in purifying steel and refining grains, as well as reasonable component ratio and process, to improve strength and grain uniformity, reduce iron loss, promote the formation of favorable texture and improve magnetic properties.
[0043] The present inventors have rationally controlled the contents of Si, Al, Mn, P and Ce within a range that is beneficial to magnetic properties through experimental research.
[0044] Embodiment 1:
[0045] The chemical composition (by weight percentage) of non-oriented electrical steel is as follows:
[0046] Table 1 Chemical composition of continuous casting slab (unit: %)
[0047] plan C Si Mn P S Al Ce 1 0.003 1.6 0.59 0.28 0.002 1.9 0.020
[0048] After smelting and continuous casting, the ingot thickness is 230mm, the hot rolling start temperature is 1100-1200℃, the final rolling temperature is 920℃, the coiling temperature is 700℃, and the steel plate thickness is 2.2mm; the normalizing temperature is 900-1000℃, and the steel coil is cold-rolled to 0.30mm after pickling. The steel coil after cold rolling is annealed in a high-temperature tubular annealing furnace with a protective gas of 80% nitrogen and 20% hydrogen, and the annealing temperature is 850-950℃. The annealed steel coil is coated with a semi-organic coating to ensure insulation and interlayer resistance. The magnetic induction intensity B of the obtained high-strength non-oriented electrical steel 50 1.71T, W 1.0 / 400 =16.7W / Kg, yield strength R el The tensile strength R is 590MPa. m It is 695MPa.
[0049] Embodiment 2:
[0050] The chemical composition (by weight percentage) of non-oriented electrical steel is as follows:
[0051] Table 2 Chemical composition of continuous casting slab (unit: %)
[0052] plan C Si Mn P S Al Ce 1 0.002 1.95 0.69 0.34 0.001 2.0 0.025
[0053] After smelting and continuous casting, the ingot thickness is 230mm, the hot rolling start temperature is 1100-1200℃, the final rolling temperature is 930℃, the coiling temperature is 710℃, the steel plate thickness is 2.2mm, the normalizing temperature is 900-1000℃, and the steel coil after pickling is cold rolled to 0.30mm. The steel coil after cold rolling is annealed in a high-temperature tubular annealing furnace with a protective gas of 80% nitrogen and 20% hydrogen, and the annealing temperature is 850-950℃. The annealed steel coil is coated with a semi-organic coating to ensure insulation and interlayer resistance. The magnetic induction intensity B of the obtained high-strength non-oriented electrical steel 50 1.68T, W 1.0 / 400 =15.5W / Kg, yield strength R el The tensile strength is 650MPa and the m It is 750MPa.
[0054] Embodiment 3:
[0055] The chemical composition (by weight percentage) of non-oriented electrical steel is as follows:
[0056] Table 3 Chemical composition of continuous casting slab (unit: %)
[0057] plan C Si Mn P S Al Ce 1 0.002 1.1 0.70 0.35 0.001 1.5 0.016
[0058] After smelting and continuous casting, the ingot thickness is 230mm, the hot rolling start temperature is 1100-1200℃, the final rolling temperature is 930℃, the coiling temperature is 690℃, and the steel plate thickness is 2.2mm; the normalizing temperature is 900-1000℃, and the steel coil is cold-rolled to 0.30mm after pickling. The steel coil after cold rolling is annealed in a high-temperature tubular annealing furnace with a protective gas of 80% nitrogen and 20% hydrogen, and the annealing temperature is 850-950℃. The annealed steel coil is coated with a semi-organic coating to ensure insulation and interlayer resistance. The magnetic induction intensity B of the obtained high-strength non-oriented electrical steel 50 1.75T, W 1.0 / 400 =17.3W / Kg, yield strength R el The tensile strength R is 580MPa. m It is 685MPa.
[0059] Embodiment 4:
[0060] The chemical composition (by weight percentage) of non-oriented electrical steel is as follows:
[0061] Table 4 Chemical composition of continuous casting slab (unit: %)
[0062] plan C Si Mn P S Al Ce 1 0.002 1.15 0.42 0.20 0.001 1.2 0.019
[0063] After smelting and continuous casting, the ingot thickness is 230mm, the hot rolling start temperature is 1100-1200℃, the final rolling temperature is 900℃, the coiling temperature is 680℃, and the steel plate thickness is 2.2mm; the normalizing temperature is 900-1000℃, and the steel coil is cold-rolled to 0.30mm after pickling. The steel coil after cold rolling is annealed in a high-temperature tubular annealing furnace with a protective gas of 80% nitrogen and 20% hydrogen, and the annealing temperature is 850-950℃. The annealed steel coil is coated with a semi-organic coating to ensure insulation and interlayer resistance. The magnetic induction intensity B of the obtained high-strength non-oriented electrical steel 50 1.73T, W 1.0 / 400 =16.5W / Kg, yield strength R el The tensile strength is 550MPa and the m It is 650MPa.
[0064] Comparative Example 1:
[0065] The chemical composition (by weight percentage) of non-oriented electrical steel is as follows:
[0066] Table 5 Chemical composition of continuous casting slab (unit: %)
[0067] plan C Si Mn P S Al Ce 1 0.002 1.0 0.38 0.18 0.001 0.85 0.012
[0068] After smelting and continuous casting, the ingot thickness is 230mm, the hot rolling start temperature is 1100-1200℃, the final rolling temperature is 940℃, the coiling temperature is 710℃, and the steel plate thickness is 2.2mm; the normalizing temperature is 900-1000℃, and the steel coil is cold-rolled to 0.30mm after pickling. The steel coil after cold rolling is annealed in a high-temperature tubular annealing furnace with a protective gas of 80% nitrogen and 20% hydrogen, and the annealing temperature is 850-950℃. The annealed steel coil is coated with a semi-organic coating to ensure insulation and interlayer resistance. The magnetic induction intensity B of the obtained non-oriented electrical steel 50 1.70T, W 1.0 / 400 =20.9W / Kg, yield strength R el The tensile strength is 420MPa and R m It is 543MPa.
[0069] Comparative Example 2:
[0070] Table 6 Chemical composition of continuous casting slab (unit: %)
[0071] plan C Si Mn P S Al Ce 1 0.002 2.2 0.78 0.40 0.001 2.1 0.040
[0072] After smelting and continuous casting, the ingot thickness is 230mm, the hot rolling start temperature is 1100-1200℃, the final rolling temperature is 905℃, the coiling temperature is 690℃, and the steel plate thickness is 2.2mm; the normalizing temperature is 900-1000℃, and the steel coil is cold-rolled to 0.30mm after pickling. The steel coil after cold rolling is annealed in a high-temperature tubular annealing furnace with a protective gas of 80% nitrogen and 20% hydrogen, and the annealing temperature is 850-950℃. The annealed steel coil is coated with a semi-organic coating to ensure insulation and interlayer resistance. The magnetic induction intensity B of the obtained non-oriented electrical steel 50 1.66T, W 1.0 / 400 =15.6W / Kg, yield strength R el The tensile strength is 560MPa and the m It is 675MPa, the plasticity of the steel plate is reduced, and rolling is difficult.
[0073] In summary, the various properties of the high-strength non-oriented electrical steel prepared in Examples 1-4 can meet the design requirements. In Comparative Example 1, the contents of Si, Mn, P, Al, and Ce are relatively low, and the percentage content is set as Si>Al. Although the magnetic induction intensity can meet the design requirements, the iron loss is high and the strength is low. In Comparative Example 2, the contents of Si, Mn, P, Al, and Ce are relatively high, and the percentage content is set as Si>Al. Although the iron loss and strength can meet the design requirements, the magnetic induction is low and the plasticity is reduced, resulting in rolling difficulties.
[0074] The above are only preferred embodiments of the present invention. It should be noted that the above preferred embodiments should not be regarded as limiting the present invention, and the protection scope of the present invention should be based on the scope defined by the claims. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the spirit and scope of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.
Claims
1. A high-strength non-oriented electrical steel with excellent magnetic properties, characterized in that: The chemical composition of the non-oriented electrical steel is as follows by weight percentage: C: 0.001-0.005%, Si: 1.1-2.0%, Mn: 0.4-0.7%, Al: 1.1-2.0%, P: 0.2-0.35%, S: ≤0.005%, Ce: 0.015-0.035%, and the balance is iron and unavoidable impurities.
2. The high-strength non-oriented electrical steel with excellent magnetic properties according to claim 1, characterized in that: The chemical composition of the non-oriented electrical steel is as follows by weight percentage: C: 0.002%, Si: 1.95%, Mn: 0.69%, Al: 2.0%, P: 0.34%, S: 0.001%, Ce: 0.025%, and the remainder is iron and inevitable impurities.
3. The high-strength non-oriented electrical steel with excellent magnetic properties according to claim 1, characterized in that: Weight ratio Mn / P≥2.
4. The high-strength non-oriented electrical steel with excellent magnetic properties according to claim 1, characterized in that: The weight percentage content Si is less than Al.
5. The high-strength non-oriented electrical steel with excellent magnetic properties according to claim 1, characterized in that: The magnetic properties of the non-oriented electrical steel are as follows: when the thickness is 0.30 mm, B 50 =1.68-1.75T, P 1.0 / 400 =15.5-19.5W / Kg, yield strength R el 550-650MPa, tensile strength R m 650-750MPa, elongation A 50 ≤20%.
6. A method for producing high-strength non-oriented electrical steel with excellent magnetic properties as claimed in any one of claims 1 to 5, characterized in that: The process includes the following steps: molten iron pretreatment → converter smelting → continuous casting → hot rolling → curling → normalizing → cold rolling → annealing → finished product.
7. The method for producing high-strength non-oriented electrical steel with excellent magnetic properties according to claim 6, characterized in that: The hot rolling start temperature is 1100-1200℃, and the hot rolling finish temperature is 900-950℃.
8. The method for producing high-strength non-oriented electrical steel with excellent magnetic properties according to claim 6, characterized in that: The curling temperature is 680-710℃.
9. The method for producing high-strength non-oriented electrical steel with excellent magnetic properties according to claim 6, characterized in that: Normalizing temperature 900-1000℃.
10. The method for producing high-strength non-oriented electrical steel with excellent magnetic properties according to claim 6, characterized in that: The annealing temperature is 850-950℃.
Citation Information
Patent Citations
Method for preparing high-magnetic induction and high-strength non-oriented silicon steel based on thin strip continuous casting
CN105803311A
Method for preparing high-strength non-oriented silicon steel based on nano Cu precipitation strengthening
CN106282781A
Manufacturing method of high-strength non-oriented silicon steel for new energy vehicle driving motor
CN106435358A
Preparation method for low-iron-loss high-strength non-oriented electrical steel
CN108286014A
High-strength non-oriented electrical steel containing rare earth and high carbon and used for new energy drive motor and manufacturing method thereof
CN111235461A
Cited By
Method for improving manufacturability of high-alloy non-oriented electrical steel
CN121653310A