Device and method for one-furnace multi-group silicon carbide single crystal growth by liquid phase method

By using seed-filled rod fixing sheets to connect multiple seed-filled rods in the liquid-phase growth furnace, the growth of multiple seed crystals is solved, and the problem of low growth efficiency of single crystals of silicon carbide in the liquid-phase growth furnace is improved and production efficiency is improved. The crystal thickness reduces the formation of flux inclusions and achieves efficient growth of silicon carbide single crystals.

CN118996604APending Publication Date: 2024-11-22TIANJIN UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411182777.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The growth of single crystals of silicon carbide in liquid phase has the problem of low production efficiency. A single crystal growth furnace can only grow one crystal ingot, with limited effective thickness and weak internal flow of the solution leading to insufficient carbon transport and component deviation, affecting the length and thickness of the crystal.

Method used

The device and method for growing single crystals of multiple groups of silicon carbide in a furnace is adopted by a liquid phase method. Multiple seed crystal growth is achieved by connecting multiple seed crystal rods in the growth furnace, thereby enhancing solution stirring and Carbon transport slows down component evaporation and improves production efficiency.

Benefits of technology

The efficient growth of single crystals of silicon carbide in liquid phase is achieved, the production efficiency is improved, the frequency of flux inclusions in the crystal is reduced, the crystal growth time is increased, the cost is reduced, and the thickness and quality of the crystal are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996604A_ABST
    Figure CN118996604A_ABST
Patent Text Reader

Abstract

The invention discloses a liquid phase method one-furnace multi-group silicon carbide single crystal growth device and a method thereof. A plurality of sub seed rods are connected by using a sub seed rod fixing sheet on a main seed crystal lifting rod in a liquid phase method growth furnace, so that a plurality of seed crystals are bonded to realize one-furnace multi-group crystal growth; and the production efficiency is improved by multiple times at the same growth time. In addition, evaporation of solution components can be slowed down by using the seed separating rod fixing piece, transportation of carbon in the solution can be enhanced by the stirring effect of the seed separating rod, the formation frequency of flux inclusion in the crystal can be reduced while polycrystal growth is achieved, the crystal growth time is prolonged as much as possible, and the yield of the crystal is increased. The device and the method provided by the invention can solve the problem of low production efficiency of the liquid-phase silicon carbide single crystal, and achieve the purposes of reducing cost and improving efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor technology, and in particular to a device and a method for growing multiple groups of silicon carbide single crystals in one furnace using a liquid phase method. Background Art

[0002] Silicon carbide is a typical wide bandgap semiconductor material and is the third generation semiconductor material after silicon and gallium arsenide. Compared with silicon and gallium arsenide, silicon carbide plays an important role in electronic devices due to its advantages such as high critical breakdown field strength, high thermal conductivity and chemical stability. It is suitable for making high-density power microelectronic devices and electronic devices working under extreme conditions such as high temperature, high frequency, high voltage and high power. Gallium nitride RF devices with high-purity semi-insulating silicon carbide as substrate are mainly used in the field of 5G communications; high-voltage and high-current power electronic devices with conductive silicon carbide as substrate can be used in large-scale substation systems, electric vehicles, charging piles and other fields.

[0003] The top seed solution growth (TSSG) method of silicon carbide crystal growth technology is a representative of the liquid phase method. Compared with the physical vapor transport (PVT) method, its growth temperature is relatively lower and closer to thermodynamic equilibrium. It is a method with the potential to grow high-quality silicon carbide single crystals. Its basic growth principle is to use a graphite crucible as a container for raw materials and as a source of carbon. When the crystal grows, carbon dissolves at the crucible wall (high temperature zone) and is transported to the seed crystal (low temperature zone) through the solution to combine with silicon to precipitate into a silicon carbide single crystal.

[0004] However, the current TSSG method of silicon carbide crystal growth has the problem of low production efficiency. On the one hand, a single crystal growth furnace only grows one ingot at a time. On the other hand, the effective thickness of a single ingot grown by a single crystal growth furnace is not large. The weak flow inside the solution may lead to insufficient carbon transport and thus cause defects such as flux inclusions. At the same time, the evaporation of the solution will also cause the composition to deviate from the ideal ratio originally designed. The reduction of certain elements that can inhibit step aggregation will also increase the probability of flux inclusion formation in the crystal, all of which affect the growth and thickness of the crystal.

[0005] The above problems lead to huge challenges in the industrial application of silicon carbide crystals grown by liquid phase method. The growth of silicon carbide crystals by liquid phase method has the advantage of expanding diameter. Although it has been reported that the diameter of silicon carbide crystals grown by liquid phase method can reach 8 inches, the thickness of 1-inch silicon carbide single crystals obtained by liquid phase method is reported to be about 30 mm, the thickness of 2-4-inch silicon carbide single crystals is between 15-20 mm, and the thickness of 8-inch silicon carbide single crystals does not exceed 5 mm. Therefore, in order to maintain the diameter expansion advantage of liquid phase method silicon carbide crystal growth while improving the production efficiency of liquid phase method silicon carbide single crystals, the present invention proposes a device and method for growing multiple groups of silicon carbide single crystals in one furnace using a liquid phase method. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a device and method for growing multiple groups of silicon carbide single crystals in one furnace by a liquid phase method, so as to at least achieve the purpose of improving the production efficiency of silicon carbide single crystals.

[0007] To solve the above technical problems, according to one aspect of the present invention, a device for growing multiple groups of silicon carbide single crystals in one furnace by a liquid phase method is provided, comprising a furnace body of a single crystal growth furnace, wherein the furnace body is provided with: - Crucible system, the crucible system includes a growth crucible and a crucible support, the growth crucible support is placed on the upper part of the crucible support, the lower end of the crucible support passes through the bottom of the furnace body and is connected to the transmission device; ——A seed crystal rod system, the seed crystal rod system includes a main seed crystal rod, a sub-seed crystal rod fixing plate, a sub-seed crystal rod and a seed crystal holder; the upper end of the main seed crystal rod passes through the top of the furnace body and is connected to the transmission device, the lower end of the main seed crystal rod extends into the growth crucible and is connected to the sub-seed crystal rod fixing plate, at least two sub-seed crystal rods are connected to the bottom of the sub-seed crystal rod fixing plate, and the lower end of the sub-seed crystal rod is connected to a seed crystal holder for bonding the seed crystal.

[0008] Furthermore, the sub-seed crystal rod fixing plate comprises a graphite annular outer ring, a graphite support frame is arranged inside the graphite annular outer ring, the main seed crystal rod is connected to the center of the graphite support frame, and each sub-seed crystal rod is evenly arranged around the center of the graphite support frame.

[0009] Furthermore, the sub-seed crystal rod fixing plate comprises a graphite disc, the main seed crystal rod is connected to the center of the graphite disc, and each sub-seed crystal rod is evenly arranged around the center of the graphite disc.

[0010] Furthermore, the furnace body includes an insulation layer, a coil and a quartz tube; the coil is arranged on the outer wall of the quartz tube, and the insulation layer includes an upper insulation layer, a side insulation layer and a lower insulation layer, wherein the side insulation layer is arranged on the inner wall of the quartz tube, and the upper insulation layer and the lower insulation layer are supported and arranged on the top and bottom of the quartz tube and the side insulation layer respectively.

[0011] Furthermore, the outer diameter of the seed crystal dividing rod fixing plate is 50-700 mm, the length of the seed crystal dividing rod is 50-200 mm, and the diameter of the seed crystal is 12-200 mm.

[0012] Furthermore, the upper insulation layer and the lower insulation layer are both solid felt, the side insulation layer is solid felt or soft felt, the solid felt is 20-200 mm thick, and the soft felt is laid in layers with a single layer thickness of 2-15 mm.

[0013] Furthermore, the growth crucible includes a crucible body and a crucible cover, the inner diameter of the crucible body is 60-800 mm, the outer height of the crucible body is 120-420 mm, the wall thickness of the crucible body is 10-40 mm, the bottom thickness of the crucible body is 10-30 mm, and the thickness of the crucible cover is 3-10 mm.

[0014] Furthermore, a temperature measuring instrument for monitoring the temperature of the bottom of the crucible is included.

[0015] According to another aspect of the present invention, a method for growing multiple groups of silicon carbide single crystals in one furnace by a liquid phase method is provided, characterized in that the method is implemented by using the above-mentioned device, and comprises: Step 1: vacuum the furnace chamber of the single crystal growth furnace, and when the pressure in the furnace chamber reaches 0.01 Pa-10 Pa, argon gas or nitrogen-argon mixed gas is injected, and the temperature is increased when the pressure in the furnace reaches 0.8-1.3 atm; Step 2: heating the growth crucible by means of a coil, from room temperature to 1600-1800°C at a heating rate of 5-30°C / min, and maintaining the temperature for 20-40 min after reaching the specified temperature for chemical reaction, and before maintaining the temperature, slowly lowering the seed crystal to a position 5-10 mm above the estimated liquid surface at a speed of 150-300 mm / h, while rotating the main seed crystal rod at a speed of 1-15 rpm and the growth crucible at a speed of 1-10 rpm, with the main seed crystal rod and the growth crucible rotating in opposite directions; Step 3: After the constant temperature material is finished, continue to heat up at a heating rate of 0.5-2 ° C / min, and at the same time, let the seed crystal rod system descend, and set its descending speed to 30-50 mm / h. According to the change of the gravity indication of the pulling system, it is judged whether the seed crystal contacts the liquid surface, until the seed crystal reaches the position 5-10 mm below the liquid surface and starts to melt back. The melting time is 10-30 min. During the melting process, the rotation speed of the main seed crystal rod is increased to 10-50 rpm, and the rotation speed of the growth crucible is increased to 5-20rpm; Step 4: After the melting is completed, the main seed crystal rod is pulled at a speed of 30-50 mm / h until the seed crystal reaches the target growth position. The temperature rises continuously during the melting and pulling process. When the temperature rises to 1700-1900 °C, the temperature is constant and the crystal growth begins. The growth time is 1-100 h. Step 5. After the growth is completed, control the main seed crystal rod to be pulled up at a speed of 30-50 mm / h until the crystal is out of the liquid surface, turn off the rotation system, set the cooling program, and cool down to room temperature at a cooling rate of 0.5-10 ℃ / min to complete the crystal growth.

[0016] Furthermore, after the growth of the silicon carbide crystal is completed, the furnace is opened, the crystal is taken out, and the surface of the crystal is corroded with hydrochloric acid and hydrofluoric acid.

[0017] The present invention provides a device and method for growing multiple groups of silicon carbide single crystals in one furnace by a liquid phase method. By using a sub-seed crystal rod fixing plate on the main seed crystal lifting rod in the liquid phase growth furnace to connect multiple sub-seed crystal rods to bond multiple seed crystals, the growth of multiple groups of crystals in one furnace is achieved, and the production efficiency is increased several times for the same growth time. In addition, the use of the sub-seed crystal rod fixing plate can slow down the evaporation of solution components, and the stirring effect of the multiple seed crystal rods can enhance the transport of carbon in the solution. The present invention can reduce the formation frequency of flux inclusions in the crystal while achieving the growth of multiple crystals, and increase the crystal growth time as much as possible. The device and method described in the present invention can solve the problem of low production efficiency of silicon carbide single crystals by the liquid phase method, and achieve the purpose of reducing costs and increasing efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a schematic structural diagram of a silicon carbide single crystal growth device provided by the present invention; Figure 2 It is a schematic diagram of a seed crystal rod fixing plate structure; Figure 3 It is a schematic diagram of another structure of a seed crystal rod fixing plate; Figure 4 This is a picture of the crystal obtained in Comparative Example 1 under an optical microscope; Figure 5 is a picture of the crystal obtained in Example 1 under an optical microscope; Figure 6 This is a picture of the crystal obtained in Example 2 under an optical microscope.

[0019] In the figure, 1-seed crystal rod system; 1-1-main seed crystal rod; 1-2-sub-seed crystal rod fixing plate; 1-3-sub-seed crystal rod; 1-4-seed crystal holder; 2-growth crucible; 2-1-crucible cover; 2-2-crucible body; 3-seed crystal; 4-crucible support; 5-insulation layer; 5-1-upper insulation layer; 5-2-side insulation layer; 5-3-lower insulation layer; 6-coil; 7-quartz tube; 8-growth raw material. DETAILED DESCRIPTION

[0020] A typical embodiment of the present invention provides a device for growing multiple groups of silicon carbide single crystals in one furnace using a liquid phase method, such as Figure 1 As shown, it includes a furnace body of a single crystal growth furnace, wherein a crucible system and a seed rod system are arranged inside the furnace body.

[0021] The crucible system comprises a growth crucible 2 and a crucible support 4. The growth crucible 2 is supported and placed on the upper part of the crucible support 4. The lower end of the crucible support 4 passes through the bottom of the furnace body and is connected to the transmission device.

[0022] The seed crystal rod system 1 includes a main seed crystal rod 1-1, a sub-seed crystal rod fixing plate 1-2, a sub-seed crystal rod 1-3 and a seed crystal holder 1-4; the upper end of the main seed crystal rod 1-1 passes through the top of the furnace body and is connected to the transmission device, the lower end of the main seed crystal rod 1-1 extends into the interior of the growth crucible 2 and is connected to the sub-seed crystal rod fixing plate 1-2, at least two sub-seed crystal rods 1-3 are connected to the bottom of the sub-seed crystal rod fixing plate 1-2, and the lower end of the sub-seed crystal rod 1-3 is connected to a seed crystal holder 1-4 for bonding the seed crystal 3.

[0023] The basic concept of this embodiment is to use a sub-seed crystal rod fixing plate 1-2 to connect multiple sub-seed crystal rods 1-3 on the main seed crystal lifting rod in the liquid phase growth furnace to bond multiple seed crystals to achieve polycrystalline growth. The stirring effect of multiple sub-seed crystal rods 1-3 can also increase solution convection and promote the transmission of carbon in the solution.

[0024] In this embodiment, the sub-seed crystal rod fixing plate 1-2 is provided with threaded holes for connecting the main seed crystal rod 1-1 and the sub-seed crystal rod 1-3, the threaded hole for connecting the main seed crystal rod 1-1 is arranged at the center of the sub-seed crystal rod fixing plate 1-2, and the threaded holes for connecting the sub-seed crystal rod 1-3 are distributed in rotational symmetry in the sub-seed crystal rod fixing plate 1-2. The number of sub-seed crystal rods 1-3 connected to the sub-seed crystal rod fixing plate 1-2 can be 2-8.

[0025] The seed crystal holder 1-4 is in the shape of a right truncated cone, the outer diameter of the upper platform of the seed crystal holder 1-4 is equal to the diameter of the seed crystal rod 1-3, and the diameter of the lower platform of the seed crystal holder 1-4 is less than or equal to the diameter of the seed crystal 3.

[0026] In this embodiment, the upper end of the crucible support 4 is a disc, and a groove is arranged in the disc for supporting and fixing the growth crucible 2 .

[0027] The present invention provides two preferred structures of seed rod fixing plates 1-2.

[0028] Among them, Figure 2 As shown, in a preferred embodiment, the sub-seed crystal rod fixing plate 1-2 includes a graphite annular outer ring, a graphite support frame is arranged inside the graphite annular outer ring, the main seed crystal rod 1-1 is connected to the center of the graphite support frame, and each sub-seed crystal rod 1-3 is evenly arranged around the center of the graphite support frame.

[0029] In another preferred embodiment, Figure 3 As shown, the sub-seed crystal rod fixing plate 1-2 comprises a graphite disk, the main seed crystal rod 1-1 is connected to the center of the graphite disk, and each sub-seed crystal rod 1-3 is evenly arranged around the center of the graphite disk. In this embodiment, the sub-seed crystal rod fixing plate 1-2 can slow down the evaporation of solution components.

[0030] In a relatively specific embodiment, the furnace body includes a thermal insulation layer 5, a coil 6 and a quartz cylinder 7. The coil 6 is arranged on the outer wall of the quartz cylinder 7, and the thermal insulation layer 5 includes an upper thermal insulation layer 5-1, a side thermal insulation layer 5-2 and a lower thermal insulation layer 5-3, wherein the side thermal insulation layer 5-2 is arranged on the inner wall of the quartz cylinder 7, and the upper thermal insulation layer 5-1 and the lower thermal insulation layer 5-3 are supported and arranged on the top and bottom of the quartz cylinder 7 and the side thermal insulation layer 5-2, respectively.

[0031] The diameter of the main seed crystal rod 1-1 is smaller than the hole diameter of the upper insulation layer 5-1 and the center of the crucible cover 2-1, the diameter of the sub-seed crystal rod fixing plate 1-2 is smaller than the inner diameter of the crucible body 2-2, the diameter of the sub-seed crystal rod 1-3 is smaller than the diameter of the seed crystal 3, and the seed crystal rod system 1 is made of graphite.

[0032] The diameters of the upper insulation 5-1 and the lower insulation 5-3 are equal to the outer diameter of the quartz tube 7, the inner diameter of the side insulation 5-2 is larger than the outer diameter of the growth crucible 2, the outer diameter of the side insulation 5-2 is smaller than the inner diameter of the coil 6, and the inner diameter of the quartz tube 7 is slightly larger than the outer diameter of the side insulation 5-2.

[0033] The growth crucible 2 includes a crucible cover 2-1 and a crucible body 2-2. The crucible cover 2-1 is placed above the crucible body 2-2, and the crucible body 2-2 contains the growth raw material 8. The coil 6 is used to heat the growth crucible 2 to melt the growth raw material 8 into a liquid state and to maintain the growth temperature of the silicon carbide crystal in the growth system. The frequency of the coil 6 is 1 kHz-100 kHz.

[0034] The diameter of the crucible cover 2-1 is equal to the outer diameter of the crucible body 2-2, the thickness of the crucible cover 2-1 is less than the wall thickness of the crucible body 2-2, and the outer diameter of the crucible body 2-2 is slightly smaller than the inner diameter of the circular groove of the crucible support 4.

[0035] The growth crucible 2 is made of graphite, and the growth raw material 8 includes silicon and metal raw materials, and the metal raw material is one or more elements such as Si, Cr, Al, Mo, Sn, Sc, Fe, Ti, Ni, and Cu.

[0036] The upper end of the main seed crystal rod 1-1 is connected to the transmission device above the single crystal growth furnace through the opening in the center of the upper insulation layer 5-1 and the opening in the center of the crucible cover 2-1, and the transmission device can control the lifting and rotation of the main seed crystal rod 1-1. The lower end of the crucible support 4 is connected to the transmission device below the single crystal growth furnace through the opening in the center of the lower insulation layer 5-3, and the transmission device is used to control the lifting and rotation of the crucible support 4. The main seed crystal rod rotates in the opposite direction to the growth crucible.

[0037] In a relatively specific implementation, the outer diameter of the seed crystal dividing rod fixing plate is 50-700 mm, the length of the seed crystal dividing rod is 50-200 mm, and the diameter of the seed crystal is 12-200 mm.

[0038] In a relatively specific implementation, the upper insulation layer and the lower insulation layer are both solid felt, the side insulation layer is solid felt or soft felt, the solid felt is 20-200 mm thick, and the soft felt is laid in layers with a single layer thickness of 2-15 mm.

[0039] In a relatively specific embodiment, the inner diameter of the crucible body is 60-800 mm, the outer height of the crucible body is 120-420 mm, the wall thickness of the crucible body is 10-40 mm, the bottom thickness of the crucible body is 10-30 mm, and the thickness of the crucible cover is 3-10 mm.

[0040] In a preferred embodiment, a thermometer for monitoring the temperature at the bottom of the crucible is also included. A circular opening is provided in the center of the crucible support 4 for the thermometer to monitor the temperature at the bottom of the crucible.

[0041] The installation steps of the above-mentioned liquid phase method one furnace multiple groups of silicon carbide single crystal growth device are as follows: In the first step, the seed crystal 3 is bonded to the seed crystal holder 1-4, the seed crystal holder 1-4 is connected to the seed crystal rod 1-3, the seed crystal rod 1-3 is connected to the seed crystal rod fixing plate 1-2, and the seed crystal rod fixing plate 1-2 is connected to the main seed crystal rod 1-1. Figure 1 shown.

[0042] The second step is to select the growth raw material used to grow silicon carbide crystals, load the growth raw material 8 into the crucible body 2-2, place the crucible body 2-2 on the crucible support 4, and adjust the temperature meter so that it can accurately detect the bottom of the growth crucible 2 through the opening in the center of the crucible support 4.

[0043] The third step is to fix the assembled seed crystal rod system 1 to the transmission device and insert the sub-seed crystal rod fixing plate 1-2 into the crucible, adjust the main seed crystal rod 1-1, so that the sub-seed crystal rod fixing plate 1-2 can rotate at the center of the crucible body 2-2 without eccentricity and without colliding with the crucible wall, and finally place the insulation layer 5 so that the lower insulation 5-3 is coaxial with the crucible support 4 and the coil 6.

[0044] Another typical embodiment of the present invention provides a method for growing multiple groups of silicon carbide single crystals in one furnace using a liquid phase method based on the device described in the above embodiment, comprising: Step 1: vacuum the furnace chamber of the single crystal growth furnace, and when the pressure in the furnace chamber reaches 0.01 Pa-10 Pa, argon gas or nitrogen-argon mixed gas is injected, and the temperature is increased when the pressure in the furnace reaches 0.8-1.3 atm; Step 2: heating the growth crucible by means of a coil, from room temperature to 1600-1800°C at a heating rate of 5-30°C / min, and maintaining the temperature for 20-40 min after reaching the specified temperature for chemical reaction, and before maintaining the temperature, slowly lowering the seed crystal to a position 5-10 mm above the estimated liquid surface at a speed of 150-300 mm / h, while rotating the main seed crystal rod at a speed of 1-15 rpm and the growth crucible at a speed of 1-10 rpm, with the main seed crystal rod and the growth crucible rotating in opposite directions; Step 3: After the constant temperature material is finished, continue to heat up at a heating rate of 0.5-2 ° C / min, and at the same time, let the seed crystal rod system descend, and set its descending speed to 30-50 mm / h. According to the change of the gravity indication of the pulling system, it is judged whether the seed crystal contacts the liquid surface, until the seed crystal reaches the position 5-10 mm below the liquid surface and starts to melt back. The melting time is 10-30 min. During the melting process, the rotation speed of the main seed crystal rod is increased to 10-50 rpm, and the rotation speed of the growth crucible is increased to 5-20rpm; Step 4: After the melting is completed, the main seed crystal rod is pulled at a speed of 30-50 mm / h until the seed crystal reaches the target growth position. The temperature rises continuously during the melting and pulling process. When the temperature rises to 1700-1900 °C, the temperature is constant and the crystal growth begins. The growth time is 1-100 h. Step 5. After the growth is completed, control the main seed crystal rod to be pulled up at a speed of 30-50 mm / h until the crystal is out of the liquid surface, turn off the rotation system, set the cooling program, and cool down to room temperature at a cooling rate of 0.5-10 ℃ / min to complete the crystal growth.

[0045] After the growth of the silicon carbide crystal is completed, the furnace is opened, the crystal is taken out, and the surface of the crystal is corroded with hydrochloric acid and hydrofluoric acid.

[0046] In this embodiment, the main seed crystal rod is placed in the center of the crucible when loading the furnace so that multiple seed crystals are evenly distributed in the crucible. Maintaining a relatively small rotation speed before the seed crystal enters the liquid surface can minimize the adverse effects on the seed crystal rod when the seed crystal collides with the solution. After the seed crystal enters the solution, increasing the seed crystal rotation speed is beneficial to the mixing of the solution and enhances the transmission of carbon in the solution.

[0047] The technical scheme claimed in the present invention is further described below by some examples. However, the examples and comparative examples are used to explain the embodiments of the present invention and do not exceed the scope of the subject matter of the present invention. The protection scope of the present invention is not limited by the examples. Unless otherwise specified, the materials and reagents used in the present invention can be obtained from commercial products in the art. Example 1

[0048] See also Figure 1As shown, in this embodiment, the device for growing a silicon carbide single crystal includes a seed crystal rod system 1, a growth crucible 2, a seed crystal 3, a crucible support 4, a heat preservation layer 5, a coil 6 and a quartz tube 7.

[0049] In this example, the seed crystal rod system 1 includes a main seed crystal rod 1-1, a sub-seed crystal rod fixing plate 1-2, a sub-seed crystal rod 1-3, and a seed crystal holder 1-4. The upper end of the main seed crystal rod 1-1 is connected to the transmission device above the single crystal growth furnace through the opening in the center of the upper insulation 5-1 and the opening in the center of the crucible cover 2-1, and the transmission device can control the lifting and rotation of the main seed crystal rod 1-1. The lower end of the main seed crystal rod 1-1 is connected to the sub-seed crystal rod fixing plate 1-2 and extends into the interior of the crucible body 2-2; the sub-seed crystal rod fixing plate 1-2 is threadedly connected to the main seed crystal rod 1-1 and the sub-seed crystal rod 1-3, and the lower end of the sub-seed crystal rod 1-3 is connected to the seed crystal holder 1-4, and the seed crystal holder 1-4 is used to bond the seed crystal 3.

[0050] The seed crystal rod system 1 is made of graphite. Part of the graphite is removed from the seed crystal rod fixing plate 1-2. The structure is as follows Figure 2 As shown, it includes a graphite annular outer ring, a graphite support frame is arranged inside the graphite annular outer ring, a main seed crystal rod 1-1 is connected to the center of the graphite support frame, and each sub-seed crystal rod 1-3 is evenly arranged around the center of the graphite support frame. The number of sub-seed crystal rods 1-3 connected to the sub-seed crystal rod fixing plate 1-2 is 4, and the distribution of the 4 seed crystals is rotationally symmetrical along the main seed crystal rod 1-1.

[0051] The growth crucible 2 includes a crucible cover 2-1 and a crucible body 2-2. The crucible cover 2-1 is placed above the crucible body 2-2. The crucible body 2-2 contains the growth raw material 8. The coil 6 is used to heat the growth crucible 2 so that the growth raw material 8 melts into a liquid state and can maintain the growth temperature of the silicon carbide single crystal in the growth system. The growth crucible 2 is placed on the crucible support 4. The disc at the upper end of the crucible support 4 is provided with a groove for supporting and fixing the growth crucible 2. The lower end of the crucible support 4 is connected to the transmission device below the single crystal growth furnace through the opening in the center of the lower insulation layer 5-3. The transmission device is used to control the lifting and rotation of the crucible support 4. A circular opening is provided in the center of the crucible support 4 for a thermometer to monitor the bottom temperature of the crucible.

[0052] The insulation layer 5 includes an upper insulation layer 5-1, a side insulation layer 5-2 and a lower insulation layer 5-3, wherein the side insulation layer 5-2 is arranged on the inner wall of the quartz tube 7, and the upper insulation layer 5-1 and the lower insulation layer 5-3 are supported and arranged on the top and bottom of the quartz tube 7 and the side insulation layer 5-2 respectively.

[0053] In this embodiment, the outer diameter of the seed crystal dividing rod fixing plate 1-2 is 150 mm, the length of the seed crystal dividing rod 1-3 is 80 mm, and the diameter of the seed crystal 3 is 35 mm.

[0054] The inner diameter of the crucible body 2-2 is 180 mm, the outer height of the crucible body 2-2 is 200 mm, the wall thickness of the crucible body 2-2 is 20 mm, the bottom thickness of the crucible body 2-2 is 20 mm, and the thickness of the crucible cover 2-1 is 8 mm.

[0055] The upper insulation 5-1 and the lower insulation 5-3 are both solid felt, and the side insulation 5-2 is soft felt. The solid felt is 70 mm thick, and the soft felt is laid in layers, with a single layer thickness of 4 mm.

[0056] In this embodiment, the metal growth raw materials include Si, Cr, and Al, the inner diameter of the coil 6 is 440 mm, and the frequency of the coil 6 is 15 kHz.

[0057] The assembly sequence of the silicon carbide single crystal growth device is: (1) The seed crystal 3 is bonded to the seed crystal holder 1-4, the seed crystal holder 1-4 is connected to the seed crystal rod 1-3, the seed crystal rod 1-3 is connected to the seed crystal rod fixing plate 1-2, and the seed crystal rod fixing plate 1-2 is connected to the main seed crystal rod 1-1.

[0058] (2) Select the growth material used to grow silicon carbide crystals, and load the growth material 8 with a molar ratio of Si:Cr:Al=0.7:0.29:0.01 into the crucible body 2-2. The crucible body 2-2 is placed on the crucible support 4. Adjust the temperature meter so that it can accurately detect the bottom of the crucible through the opening in the center of the crucible support 4.

[0059] (3) Fix the assembled seed crystal rod system 1 to the transmission device and insert the sub-seed crystal rod fixing plate 1-2 into the crucible. Adjust the main seed crystal rod 1-1 so that the sub-seed crystal rod fixing plate 1-2 can rotate in the center of the crucible body 2-2 without eccentricity and without colliding with the crucible wall. Finally, place the insulation layer 5 so that the lower insulation 5-3 is coaxial with the crucible support 4 and the coil 6.

[0060] The liquid phase growth device for silicon carbide crystal in this embodiment is used to grow silicon carbide crystal by liquid phase method, including the following steps: (1) After the furnace is loaded, the furnace chamber is evacuated. When the pressure in the furnace chamber reaches 0.1 Pa, argon gas is injected. When the pressure in the furnace reaches 1.3 atm, the temperature begins to rise.

[0061] (2) The growth crucible 2 is heated by the coil 6 at a heating rate of 12°C / min to 1680°C. After reaching the specified temperature, the temperature is maintained at a constant temperature for 25 min for chemical reaction. Before the temperature is maintained at a constant temperature, the seed crystal 3 is slowly lowered at a speed of 300 mm / h to a position 10 mm above the estimated liquid surface. At the same time, the main seed crystal rod 1-1 is rotated at a speed of 5 rpm and the growth crucible 2 is rotated at a speed of 3 rpm. The rotation direction of the main seed crystal rod 1-1 is opposite to that of the growth crucible 2.

[0062] (3) After the constant temperature material is finished, continue to heat up at a rate of 1.5 °C / min, and at the same time, let the seed crystal rod system 1 descend, and set its descending speed to 50 mm / h. According to the change of the gravity indication of the pulling system, it is judged whether the seed crystal 3 contacts the liquid surface, until the seed crystal 3 reaches the position 10 mm below the liquid surface and starts to melt back. The melting time is 15 min. During the melting process, the rotation speed of the main seed crystal rod is slowly increased to 40 rpm, and the rotation speed of the crucible is slowly increased to 15 rpm.

[0063] (4) After the remelting is completed, the main seed crystal rod 1-1 is pulled at a speed of 50 mm / h until the seed crystal 3 reaches the target growth position. The temperature continues to rise during the remelting and pulling process. When the temperature rises to 1800 °C and stabilizes, crystal growth begins. The growth time is 5 hours.

[0064] (5) After the growth is completed, the main seed crystal rod 1-1 is controlled to be pulled up at a speed of 50 mm / h until the crystal is out of the liquid surface, the rotation system is turned off, and a cooling program is set to cool down to room temperature at a cooling rate of 2 °C / min to complete the crystal growth.

[0065] (6) Open the furnace, take out the grown crystals, corrode the crystal surface with hydrochloric acid and hydrofluoric acid, and then observe the crystal surface morphology under an optical microscope. Example 2

[0066] The difference from Example 1 is only that Figure 3 The sub-seed crystal rod fixing plate 1-2 shown in the figure comprises an integral graphite disc, the main seed crystal rod 1-1 is connected to the center of the graphite disc, and the sub-seed crystal rods 1-3 are evenly arranged around the center of the graphite disc. Example 3

[0067] The only difference from Example 1 is that in this embodiment, the outer diameter of the seed crystal rod fixing plate 1-2 is 50 mm, the length of the seed crystal rod 1-3 is 50 mm, and the diameter of the seed crystal 3 is 12 mm.

[0068] The inner diameter of the crucible body 2-2 is 60 mm, the outer height of the crucible body 2-2 is 120 mm, the wall thickness of the crucible body 2-2 is 10 mm, the bottom thickness of the crucible body 2-2 is 10 mm, and the thickness of the crucible cover 2-1 is 3 mm.

[0069] The upper insulation 5-1 and the lower insulation 5-3 are both solid felt, and the side insulation 5-2 is soft felt. The solid felt is 20 mm thick, and the soft felt is laid in layers, with a single layer thickness of 2 mm.

[0070] In this embodiment, the metal growth raw materials include Si, Cr, and Al, the inner diameter of the coil 6 is 120 mm, and the frequency of the coil 6 is 15 kHz. Example 4

[0071] The only difference from Example 2 is that in this embodiment, the diameter of the seed crystal rod fixing plate 1-2 is 700 mm, the length of the seed crystal rod 1-3 is 200 mm, and the diameter of the seed crystal 3 is 200 mm.

[0072] The inner diameter of the crucible body 2-2 is 800 mm, the outer height of the crucible body 2-2 is 420 mm, the wall thickness of the crucible body 2-2 is 40 mm, the bottom thickness of the crucible body 2-2 is 30 mm, and the thickness of the crucible cover 2-1 is 10 mm.

[0073] The upper insulation 5-1, the lower insulation 5-3 and the side insulation 5-2 are all solid felts, the thickness of the solid felts is 200 mm, and the soft felts are laid in layers, and the thickness of a single layer is 15 mm.

[0074] In this embodiment, the metal growth raw materials include Si, Cr, and Al, the inner diameter of the coil 6 is 1400 mm, and the frequency of the coil 6 is 15 kHz. Example 5

[0075] The liquid phase growth device for silicon carbide crystal in the first embodiment is used, but the difference lies in that the reaction conditions for liquid phase silicon carbide crystal growth are different.

[0076] (1) After the furnace is loaded, the furnace chamber is evacuated. When the pressure in the furnace chamber reaches 0.01 pa, argon gas is injected. When the pressure in the furnace reaches 0.8 atm, the temperature begins to rise.

[0077] (2) The growth crucible 2 is heated by the coil 6 at a heating rate of 5°C / min to 1600°C. After reaching the specified temperature, the temperature is maintained at a constant temperature for 20 min for chemical reaction. Before the temperature is maintained at a constant temperature, the seed crystal 3 is slowly lowered at a speed of 150 mm / h to a position 5 mm above the estimated liquid surface. At the same time, the main seed crystal rod 1-1 is rotated at a speed of 1 rpm, and the growth crucible 2 is rotated at a speed of 1 rpm. The rotation direction of the main seed crystal rod 1-1 is opposite to that of the growth crucible 2.

[0078] (3) After the constant temperature material is finished, continue to heat up at a rate of 2°C / min, and at the same time, let the seed crystal rod system 1 descend, and set its descending speed to 30 mm / h. According to the change of the gravity indication of the pulling system, it is judged whether the seed crystal 3 contacts the liquid surface, until the seed crystal 3 reaches the position 5 mm below the liquid surface and starts to melt back. The melting time is 10 min. During the melting process, the rotation speed of the main seed crystal rod is slowly increased to 10 rpm, and the rotation speed of the crucible is slowly increased to 5 rpm.

[0079] (4) After the remelting is completed, the main seed crystal rod 1-1 is pulled at a speed of 30 mm / h until the seed crystal 3 reaches the target growth position. The temperature continues to rise during the remelting and pulling process. When the temperature rises to 1700 °C and stabilizes, crystal growth begins. The growth time is 1 hour.

[0080] (5) After the growth is completed, the main seed crystal rod 1-1 is controlled to be pulled up at a speed of 30 mm / h until the crystal is out of the liquid surface, the rotation system is turned off, and a cooling program is set to cool down to room temperature at a cooling rate of 0.5 ℃ / min to complete the crystal growth.

[0081] (6) Open the furnace, take out the grown crystals, corrode the crystal surface with hydrochloric acid and hydrofluoric acid, and then observe the crystal surface morphology under an optical microscope. Example 6

[0082] The liquid phase growth device for silicon carbide crystal in the second embodiment is used, but the difference lies in that the reaction conditions for the liquid phase method of silicon carbide crystal growth are different.

[0083] (1) After the furnace is loaded, the furnace chamber is evacuated. When the pressure in the furnace chamber reaches 10 Pa, a nitrogen-argon mixed gas is injected. When the pressure in the furnace reaches 1.3 atm, the temperature begins to rise.

[0084] (2) The growth crucible 2 is heated by the coil 6 at a heating rate of 30°C / min to 1800°C. After reaching the specified temperature, the temperature is maintained at a constant temperature for 40 min for chemical reaction. Before the temperature is maintained at a constant temperature, the seed crystal 3 is slowly lowered at a speed of 300 mm / h to a position 10 mm above the estimated liquid surface. At the same time, the main seed crystal rod 1-1 is rotated at a speed of 15 rpm and the growth crucible 2 is rotated at a speed of 10 rpm. The rotation direction of the main seed crystal rod 1-1 is opposite to that of the growth crucible 2.

[0085] (3) After the constant temperature material is finished, continue to heat up at a rate of 0.5℃ / min, and at the same time, let the seed crystal rod system 1 descend, and set its descending speed to 50 mm / h. According to the change of the gravity indication of the pulling system, it is judged whether the seed crystal 3 contacts the liquid surface, until the seed crystal 3 reaches the position 10 mm below the liquid surface and starts to melt back. The melting time is 30 minutes. During the melting process, the rotation speed of the main seed crystal rod is slowly increased to 50rpm, and the rotation speed of the crucible is slowly increased to 20rpm.

[0086] (4) After the remelting is completed, the main seed crystal rod 1-1 is pulled at a speed of 50 mm / h until the seed crystal 3 reaches the target growth position. The temperature continues to rise during the remelting and pulling process. When the temperature rises to 1900 °C and stabilizes, crystal growth begins. The growth time is 100 h.

[0087] (5) After the growth is completed, the main seed crystal rod 1-1 is controlled to be pulled up at a speed of 50 mm / h until the crystal is out of the liquid surface, the rotation system is turned off, and a cooling program is set to cool down to room temperature at a cooling rate of 10 ℃ / min to complete the crystal growth.

[0088] (6) Open the furnace, take out the grown crystals, corrode the crystal surface with hydrochloric acid and hydrofluoric acid, and then observe the crystal surface morphology under an optical microscope.

[0089] Comparative Example 1 The difference between this comparative example and Example 1 is that the seed crystal rod fixing piece 1-2 is connected to the seed crystal rod 1-3 at its center, and the number of seed crystal rods 1-3 connected to the seed crystal rod fixing piece 1-2 is 1. The crystal growth method is the same as that of Example 1.

[0090] The liquid phase silicon carbide crystal growth device selected in this comparative example is similar to most of the liquid phase growth devices currently in use. This method can only grow one crystal ingot in a single furnace, compared with the single furnace in Examples 1 and 2 that can grow four crystal ingots. The production efficiency is relatively low. In addition, in the commonly used crystal growth devices, there are often problems such as weak solution flow and serious evaporation of solution components, which leads to the appearance of cracks on the surface of the growing crystal. Figure 4The less ideal step morphology shown in the figure, Example 1 adopts the method of polycrystalline growth to enhance the solution flow and reduce the number of high steps, such as Figure 5 As shown, the graphite structure used in Example 2 inhibits the evaporation of the solution components, and the solution components can be close to the ideal ratio designed initially for a long time, the growth surface morphology is further improved, and the step distribution of the growth interface is more uniform, as shown in FIG. Figure 6 shown.

Claims

1. A device for growing multiple groups of silicon carbide single crystals in one furnace by a liquid phase method, comprising a furnace body of a single crystal growth furnace, Features: The furnace is equipped with: - Crucible system, the crucible system includes a growth crucible and a crucible support, the growth crucible support is placed on the upper part of the crucible support, the lower end of the crucible support passes through the bottom of the furnace body and is connected to the transmission device; ——A seed crystal rod system, the seed crystal rod system includes a main seed crystal rod, a sub-seed crystal rod fixing plate, a sub-seed crystal rod and a seed crystal holder; the upper end of the main seed crystal rod passes through the top of the furnace body and is connected to the transmission device, the lower end of the main seed crystal rod extends into the growth crucible and is connected to the sub-seed crystal rod fixing plate, at least two sub-seed crystal rods are connected to the bottom of the sub-seed crystal rod fixing plate, and the lower end of the sub-seed crystal rod is connected to a seed crystal holder for bonding the seed crystal.

2. The device for growing multiple groups of silicon carbide single crystals in one furnace by a liquid phase method according to claim 1, Features: The sub-seed crystal rod fixing plate comprises a graphite annular outer ring, a graphite support frame is arranged inside the graphite annular outer ring, the main seed crystal rod is connected to the center of the graphite support frame, and each sub-seed crystal rod is evenly arranged around the center of the graphite support frame.

3. The device for growing multiple groups of silicon carbide single crystals in one furnace by a liquid phase method according to claim 1, Features: The sub-seed crystal rod fixing plate comprises a graphite disc, the main seed crystal rod is connected to the center of the graphite disc, and each sub-seed crystal rod is evenly arranged around the center of the graphite disc.

4. The device for growing multiple groups of silicon carbide single crystals in one furnace by a liquid phase method according to claim 1, 2 or 3, Features: The furnace body includes an insulation layer, a coil and a quartz tube; the coil is arranged on the outer wall of the quartz tube, and the insulation layer includes an upper insulation layer, a side insulation layer and a lower insulation layer, wherein the side insulation layer is arranged on the inner wall of the quartz tube, and the upper insulation layer and the lower insulation layer are supported and arranged on the top and bottom of the quartz tube and the side insulation layer respectively.

5. The device for growing multiple groups of silicon carbide single crystals in one furnace by a liquid phase method according to claim 4, Features: The outer diameter of the seed crystal dividing rod fixing plate is 50-700 mm, the length of the seed crystal dividing rod is 50-200 mm, and the diameter of the seed crystal is 12-200 mm.

6. The device for growing multiple groups of silicon carbide single crystals in one furnace by a liquid phase method according to claim 5, Features: The upper insulation layer and the lower insulation layer are both solid felt, and the side insulation layer is solid felt or soft felt. The solid felt is 20-200 mm thick, and the soft felt is laid in layers, with a single layer thickness of 2-15 mm.

7. The device for growing multiple groups of silicon carbide single crystals in one furnace by a liquid phase method according to claim 6, Features: The growth crucible comprises a crucible body and a crucible cover. The inner diameter of the crucible body is 60-800 mm, the outer height of the crucible body is 120-420 mm, the wall thickness of the crucible body is 10-40 mm, the bottom thickness of the crucible body is 10-30 mm, and the thickness of the crucible cover is 3-10 mm.

8. The device for growing multiple groups of silicon carbide single crystals in one furnace by a liquid phase method according to claim 1 or 7, Features: Includes a thermometer for monitoring the crucible bottom temperature.

9. A method for growing multiple groups of silicon carbide single crystals in one furnace using a liquid phase method. It is characterized in that The method is implemented by using the device according to any one of claims 1 to 8, comprising: Step 1: vacuum the furnace chamber of the single crystal growth furnace, and when the pressure in the furnace chamber reaches 0.01 Pa-10 Pa, argon gas or nitrogen-argon mixed gas is injected, and the temperature is increased when the pressure in the furnace reaches 0.8-1.3 atm; Step 2: heating the growth crucible by means of a coil, from room temperature to 1600-1800°C at a heating rate of 5-30°C / min, and maintaining the temperature for 20-40 min after reaching the specified temperature for chemical reaction, and before maintaining the temperature, slowly lowering the seed crystal to a position 5-10 mm above the estimated liquid surface at a speed of 150-300 mm / h, while rotating the main seed crystal rod at a speed of 1-15 rpm and the growth crucible at a speed of 1-10 rpm, with the main seed crystal rod and the growth crucible rotating in opposite directions; Step 3: After the constant temperature material is finished, continue to heat up at a heating rate of 0.5-2 ° C / min, and at the same time, let the seed crystal rod system descend, and set its descending speed to 30-50 mm / h. According to the change of the gravity indication of the pulling system, it is judged whether the seed crystal contacts the liquid surface, until the seed crystal reaches the position 5-10 mm below the liquid surface and starts to melt back. The melting time is 10-30 min. At the same time, the rotation speed of the main seed crystal rod is increased to 10-50 rpm, and the rotation speed of the growth crucible is increased to 5-20rpm; Step 4: After the melting is completed, the main seed crystal rod is pulled at a speed of 30-50 mm / h until the seed crystal reaches the target growth position. The temperature rises continuously during the melting and pulling process. When the temperature rises to 1700-1900 °C, the temperature is constant and the crystal growth begins. The growth time is 1-100 h. Step 5. After the growth is completed, control the main seed crystal rod to be pulled up at a speed of 30-50 mm / h until the crystal is out of the liquid surface, turn off the rotation system, set the cooling program, and cool down to room temperature at a cooling rate of 0.5-10 ℃ / min to complete the crystal growth.

10. The method for growing multiple groups of silicon carbide single crystals in one furnace by a liquid phase method according to claim 1, Features: After the growth of the silicon carbide crystal is completed, the furnace is opened, the crystal is taken out, and the surface of the crystal is corroded with hydrochloric acid and hydrofluoric acid.

Citation Information

Cited By

  • N-type silicon carbide crystal and liquid phase growth method thereof

    CN120945487A

  • Device and method for simultaneously growing multiple liquid phase epitaxial wafers

    CN121629502A