Macroporous alumina and preparation method thereof

By using components such as potassium carbonate, urea/carboxy surfactant conjugates and triethoxysilane, the pore structure of macroporous alumina is adjusted, which solves the problem of difficulty in controlling pore structure and process complexity, and improves the catalytic performance and Structural stability achieves efficient catalytic and adsorption effects.

CN119018919AActive Publication Date: 2024-11-26YUEYANG HUIJING NEW MATERIAL TECH CO LTD

Patent Information

Application Number
CN202411511739.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-28
Publication Date
2024-11-26
Estimated Expiration
2044-10-28

AI Technical Summary

Technical Problem

In the preparation process of existing macroporous alumina, the pore structure is difficult to regulate, the process is complex and the cost is high, which leads to pore structures that are prone to collapse during high-temperature roasting, reducing the catalytic or adsorption effect, and limiting its application in catalysis, adsorption and other fields.

Method used

Using potassium carbonate, urea/carboxy surfactant conjugates, triethoxysilane and ethyl acetate as key components, a unique structural grid is formed by regulating the interaction between solvents and surfactants, using urea and carbonic acid Potassium produces gas to expand the pore size during high temperature calcination, and improves catalytic performance with triethoxysilane modification.

Benefits of technology

It significantly improves the pore structure and performance of macroporous alumina, ensures the uniformity of pore size and porosity, enhances the contact time of catalytic active sites and reactants, improves the catalytic conversion rate and the structural stability of the material, and extends the catalyst life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119018919A_ABST
    Figure CN119018919A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of inorganic materials, in particular to macroporous aluminum oxide and a preparation method thereof. The synthetic raw materials of the macroporous alumina comprise the following components: potassium carbonate, ethyl acetate, low-carbon alcohol, urea / carboxyl surfactant conjugate, aluminum salt, triethylamine, triethoxysilane, cane sugar and water. The urea / carboxyl surfactant conjugate is formed by coupling a carboxyl surfactant and urea through EDC / NHS. The macroporous alumina with high specific surface area and excellent pore distribution is prepared under the combined action of key components of potassium carbonate, ethyl acetate and urea / carboxyl surfactant conjugate, and the preparation method is simple in process, suitable for large-scale production and wide in application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of inorganic materials, and in particular to macroporous alumina and a preparation method thereof. Background Art

[0002] Macroporous alumina is an aluminum oxide material with a macroporous structure, and its pore size is usually between 50 nanometers and several micrometers. This material can significantly increase the specific surface area and permeability of the material by controlling the pore size and porosity, while maintaining excellent mechanical strength and chemical stability.

[0003] Due to its high specific surface area and good pore distribution, macroporous alumina is widely used in catalysis, adsorption, filtration, sensing and other fields. As a catalyst carrier, it can improve the mass transfer efficiency and catalytic activity of reactants in the fields of petrochemicals, environmental protection, etc. In terms of adsorption materials, it can effectively adsorb pollutants such as organic molecules and heavy metals, and is used in scenarios such as water treatment and air purification. In addition, due to its high temperature resistance and corrosion resistance, macroporous alumina is also an ideal choice for high-temperature filtration materials and gas sensors, especially in extreme conditions, where it can maintain the stability of its structure and performance.

[0004] The pore structure of macroporous alumina can be precisely controlled by template method, sol-gel method, bio-template method and other techniques to form a complex porous network. However, the existing technology still has some shortcomings in its preparation process. For example, it is difficult to precisely control the pore structure, especially to ensure the multi-level pore structure while maintaining the structural properties of the material. In addition, the preparation process is complicated and costly, which limits the economic feasibility of its large-scale application, and high-temperature calcination can easily cause the pore structure to collapse or deform, reduce the specific surface area, and ultimately weaken its catalytic or adsorption effect. Therefore, the development of more efficient synthesis technology is still a major challenge facing current technology. Summary of the invention

[0005] In view of the above situation, in order to overcome the defects of the prior art, the present invention provides a macroporous alumina and a preparation method thereof.

[0006] In order to achieve the above-mentioned purpose, the technical scheme adopted by the present invention is as follows: The present invention proposes a macroporous alumina, and the raw materials for synthesizing the macroporous alumina include the following components: potassium carbonate, ethyl acetate, low-carbon alcohol, urea / carboxyl surfactant conjugate, aluminum salt, triethylamine, triethoxysilane, sucrose and water.

[0007] Preferably, the method for preparing the urea / carboxyl surfactant conjugate comprises the following steps: A1. Dissolve 0.1 mol of urea in 100 mL of anhydrous ethanol, stir until completely dissolved, add 0.12 mol of acetic anhydride, and add 0.6 mL of anhydrous pyridine, stir and react at room temperature for 2-4 hours. After the reaction is completed, pour the reaction mixture into 0°C ether solution, centrifuge, take the precipitate, wash with ether, and obtain acetylated urea; A2, add 0.1 mol of carboxyl surfactant to 100 mL of ethanol, stir to completely dissolve, then add 0.11 mol of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride (EDC), stir at 500 rpm for 3 h, after the reaction, add 0.11 mol of N-hydroxysuccinimide (NHS), stir at 500 rpm for 3 h to obtain an activated solution; A3. Dissolve the acetylated urea prepared in step A1 in 100 mL of deionized water, heat in a water bath at 50°C with stirring for 4 h, cool to room temperature, and then slowly add the solution to the activation solution prepared in step A2. Stir the mixture at 400-600 rpm at 30-35°C for 6-12 h. After the reaction is completed, the product is obtained. The product is extracted with dichloromethane, and then placed in a rotary evaporator to evaporate the dichloromethane. After complete evaporation, a urea / carboxyl surfactant conjugate is obtained.

[0008] Preferably, the carboxyl surfactant in step A2 is any one of stearic acid, oleic acid, palmitic acid, capric acid and sodium laurate.

[0009] Preferably, the low-carbon alcohol is any one of methanol, ethanol, n-propanol and isopropanol.

[0010] Preferably, the aluminum salt is any one of aluminum chloride, aluminum nitrate and aluminum sulfate.

[0011] The present invention also provides a method for preparing macroporous alumina, which specifically comprises the following steps: S1. Weigh 100-200 mg of urea / carboxyl surfactant conjugate and add it to 10 mL of water. Stir until completely dissolved to obtain a surfactant solution. Weigh aluminum salt and add it to water. Dissolve evenly to prepare a 1-2 mol / L aluminum salt solution. S2, add 1-2 g potassium carbonate, 5-10 mL low-carbon alcohol, 10-20 mL ethyl acetate, 0.5-2 g sucrose and 90-100 mL water into a 150 mL container, stir and disperse evenly, continue to add the surfactant solution prepared in step S1, stir and disperse evenly, and obtain a mixed solution; S3, adding 40 mL of aluminum salt solution dropwise to the mixed solution prepared in step S2, stirring at 400-600 rpm for 3-6 hours to form a uniform emulsion, continuing to add 4-6 mL of triethylamine and 2-5 mL of triethoxysilane, continuing to stir for 30-60 minutes, and standing for 6-12 hours after the reaction is completed to obtain a sol solution; S4, placing the sol solution prepared in step S3 in an oven at 60° C. and drying for 4-6 h, then heating to 80° C. and drying until the sol solution is completely free of moisture to obtain a solid precursor; S5. Place the solid precursor obtained in step S4 in a muffle furnace, heat it to 500-700°C at a heating rate of 5-10°C / min under the protection of a nitrogen flow at a flow rate of 1 L / min, maintain it for 3-5 hours, and obtain the product after naturally cooling to room temperature. Wash the product three times with water and ethanol alternately, and obtain macroporous alumina after drying.

[0012] The beneficial effects of the present invention are as follows: The present invention significantly improves the pore structure and performance of macroporous alumina by innovatively using potassium carbonate, urea / carboxyl surfactant conjugate, triethoxysilane and ethyl acetate as key components for synthesizing macroporous alumina. Specifically, ethyl acetate plays a key role as a mixed solvent. It disrupts the uniformity of the solution during the mixing process through its solvent properties, forming a unique structural grid. This grid structure not only helps to form preliminary pores, but also works together with the surfactant to ensure the formation of larger pores in the solid precursor. This method effectively optimizes the size and distribution of pores by regulating the interaction between the solvent and the surfactant.

[0013] In addition, the conjugate of urea and carboxyl surfactant plays an important role in the high-temperature calcination process. Urea decomposes to generate ammonia and carbon dioxide when heated. These gases generate pressure in the solid precursor, thereby further expanding the pore size; the decomposition of urea combined with the action of the surfactant enhances the pore expansion effect and ensures the porosity and pore size uniformity of the final material. The addition of potassium carbonate further enhances the pore size expansion. During the high-temperature calcination process, potassium carbonate decomposes to release potassium vapor and carbon dioxide. These gases generate pressure inside the solid precursor, effectively promoting the expansion of pores. This process not only enhances the generation of pore size, but also optimizes the distribution and structural stability of pores. Large porosity and high specific surface area provide more active sites for catalytic reactions, while increasing the contact time of reactants and improving catalytic conversion. For heterogeneous catalysts, large specific surface area can accommodate more catalytic active centers, thereby enhancing the catalytic effect. Due to the effect of potassium carbonate, the distribution and structure of the pores are optimized, and the structural stability of the material is also enhanced; especially when the catalytic reaction is carried out at high temperature, the pore structure of the catalyst can be effectively prevented from collapsing, thereby extending the life of the catalyst. The present invention introduces triethoxysilane modification to form a protective layer through the hydrolysis and condensation of silicon oxide, thereby improving the catalytic performance of macroporous alumina, especially the selectivity and stability in acid-base catalytic reactions. By optimizing the pore structure and surface chemical properties, the addition of triethoxysilane can effectively enhance the reaction efficiency and life of the catalyst. The present invention introduces a small amount of carbon source material sucrose into the precursor solution, removes the carbon source by calcination to produce additional pore structure, and further expands the porosity and specific surface area; at the same time, the gas generated by the decomposition of the carbon source contributes to pore formation and increases the mechanical strength of the material.

[0014] In summary, the present invention innovatively improves the pore structure of macroporous alumina by combining the comprehensive effects of ethyl acetate, urea / carboxyl surfactant conjugate, triethoxysilane and potassium carbonate. This method not only effectively expands the pore size, but also ensures the uniform distribution of pores and the structural properties of the material, providing a new technical path for the preparation of macroporous alumina. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only for the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0016] Figure 1 is a scanning electron microscope image of the macroporous alumina prepared in Example 1 of the present invention; Figure 2 is a scanning electron microscope image of the macroporous alumina prepared in Example 2 of the present invention; Figure 3 is a scanning electron microscope image of the macroporous alumina prepared in Example 3 of the present invention; Figure 4 is a scanning electron microscope image of the macroporous alumina prepared in Comparative Example 1 of the present invention; Figure 5 is a scanning electron microscope image of the macroporous alumina prepared in Comparative Example 2 of the present invention; Figure 6 is a scanning electron microscope image of the macroporous alumina prepared in Comparative Example 3 of the present invention; Figure 7 This is the XRD diagram of the macroporous alumina prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0017] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. It should be noted that, unless otherwise specified, the raw materials involved in the present invention are purchased through conventional commercial channels.

[0018] Example 1: This example proposes a macroporous alumina, wherein the raw materials for synthesizing the macroporous alumina include the following components: potassium carbonate, ethyl acetate, ethanol, urea / sodium laurate conjugate, aluminum chloride, triethylamine and water.

[0019] The preparation method of the urea / sodium laurate conjugate comprises the following steps: A1. Dissolve 0.1 mol of urea in 100 mL of anhydrous ethanol, stir until completely dissolved, add 0.12 mol of acetic anhydride, and add 0.6 mL of anhydrous pyridine, stir and react at room temperature for 2-4 hours. After the reaction is completed, pour the reaction mixture into 0°C ether solution, centrifuge, take the precipitate, wash with ether, and obtain acetylated urea; A2, add 0.1 mol of sodium laurate to 100 mL of ethanol, stir until completely dissolved, then add 0.11 mol of EDC, stir at 500 rpm for 3 h, then add 0.11 mol of NHS after the reaction, stir at 500 rpm for 3 h to obtain an activated solution; A3. Dissolve the acetylated urea prepared in step A1 in 100 mL of deionized water, heat in a water bath at 50°C with stirring for 4 h, cool to room temperature, and then slowly add the solution to the activation solution prepared in step A2. Stir the mixture at 400-600 rpm at 30-35°C for 6-12 h. After the reaction is completed, the product is obtained. The product is extracted with dichloromethane, and then placed in a rotary evaporator to evaporate the dichloromethane. After complete evaporation, urea / sodium laurate conjugate is obtained.

[0020] This embodiment also provides a method for preparing macroporous alumina, which specifically comprises the following steps: S1. Weigh 200 mg of urea / sodium laurate conjugate and add it to 10 mL of water. Stir until completely dissolved to obtain a surfactant solution. Weigh aluminum chloride and add it to water. Dissolve evenly to prepare a 2 mol / L aluminum chloride solution. S2, add 2 g potassium carbonate, 10 mL ethanol, 15 mL ethyl acetate, 2 g sucrose and 100 mL water into a 150 mL container, stir and disperse evenly, continue to add the surfactant solution prepared in step S1, stir and disperse evenly, and obtain a mixed solution; S3, adding 40 mL of aluminum chloride solution dropwise to the mixed solution prepared in step S2, stirring at 400 rpm for 6 h to form a uniform emulsion, continuing to add 6 mL of triethylamine and 5 mL of triethoxysilane, continuing to stir for 60 min, and standing for 12 h after the reaction is completed to obtain a sol solution; S4, placing the sol solution prepared in step S3 in an oven at 60° C. and drying for 6 h, then heating to 80° C. and drying until the sol solution is completely free of moisture to obtain a solid precursor; S5. Place the solid precursor obtained in step S4 in a muffle furnace, and heat it to 700°C at a heating rate of 10°C / min under the protection of a nitrogen flow at a flow rate of 1 L / min, and maintain it for 3 hours. After naturally cooling to room temperature, obtain the product, wash the product three times with water and ethanol alternately, and obtain macroporous alumina after drying.

[0021] Example 2: This example proposes a macroporous alumina, wherein the raw materials for synthesizing the macroporous alumina include the following components: potassium carbonate, ethyl acetate, methanol, urea / oleic acid conjugate, aluminum nitrate, triethylamine and water.

[0022] The preparation method of the urea / oleic acid conjugate comprises the following steps: A1. Dissolve 0.1 mol of urea in 100 mL of anhydrous ethanol, stir until completely dissolved, add 0.12 mol of acetic anhydride, and add 0.6 mL of anhydrous pyridine, stir and react at room temperature for 2-4 hours. After the reaction is completed, pour the reaction mixture into 0°C ether solution, centrifuge, take the precipitate, wash with ether, and obtain acetylated urea; A2. Add 0.1 mol of oleic acid to 100 mL of ethanol, stir until completely dissolved, then add 0.11 mol of EDC, stir at 500 rpm for 3 h, then add 0.11 mol of NHS, stir at 500 rpm for 3 h to obtain an activated solution. A3. Dissolve the acetylated urea prepared in step A1 in 100 mL of deionized water, heat in a water bath at 50°C with stirring for 4 h, cool to room temperature, and then slowly add the solution to the activation solution prepared in step A2. Stir the mixture at 400-600 rpm at 30-35°C for 6-12 h. After the reaction is completed, the product is obtained. The product is extracted with dichloromethane, and then placed in a rotary evaporator to evaporate the dichloromethane. After complete evaporation, urea / oleic acid conjugate is obtained.

[0023] This embodiment also provides a method for preparing macroporous alumina, which specifically comprises the following steps: S1. Weigh 150 mg of urea / oleic acid conjugate and add it to 10 mL of water. Stir until completely dissolved to obtain a surfactant solution. Weigh aluminum nitrate and add it to water. Dissolve evenly to prepare a 1.5 mol / L aluminum nitrate solution. S2, add 1 g potassium carbonate, 8 mL methanol, 20 mL ethyl acetate, 0.5 g sucrose and 90 mL water into a 150 mL container, stir and disperse evenly, continue to add the surfactant solution prepared in step S1, stir and disperse evenly, and obtain a mixed solution; S3, adding 40 mL of aluminum nitrate solution dropwise to the mixed solution prepared in step S2, stirring at 600 rpm for 3 h to form a uniform emulsion, continuing to add 4 mL of triethylamine and 2 mL of triethoxysilane, continuing to stir for 40 min, and standing for 6 h after the reaction is completed to obtain a sol solution; S4, placing the sol solution prepared in step S3 in an oven at 60° C. and drying for 4 h, then heating to 80° C. and drying until the sol solution is completely free of moisture to obtain a solid precursor; S5. Place the solid precursor obtained in step S4 in a muffle furnace, and heat it to 500°C at a heating rate of 5°C / min under the protection of a nitrogen flow at a flow rate of 1 L / min, and maintain it for 4 hours. After naturally cooling to room temperature, obtain the product, wash the product three times with water and ethanol alternately, and obtain macroporous alumina after drying.

[0024] Example 3: This example proposes a macroporous alumina, wherein the raw materials for synthesizing the macroporous alumina include the following components: potassium carbonate, ethyl acetate, n-propanol, urea / stearic acid conjugate, aluminum sulfate, triethylamine and water.

[0025] The preparation method of the urea / stearic acid conjugate comprises the following steps: A1. Dissolve 0.1 mol of urea in 100 mL of anhydrous ethanol, stir until completely dissolved, add 0.12 mol of acetic anhydride, and add 0.6 mL of anhydrous pyridine, stir and react at room temperature for 2-4 hours. After the reaction is completed, pour the reaction mixture into 0°C ether solution, centrifuge, take the precipitate, wash with ether, and obtain acetylated urea; A2. Add 0.1 mol of stearic acid to 100 mL of ethanol, stir until completely dissolved, then add 0.11 mol of EDC, stir at 500 rpm for 3 h, then add 0.11 mol of NHS, stir at 500 rpm for 3 h to obtain an activated solution. A3. Dissolve the acetylated urea prepared in step A1 in 100 mL of deionized water, heat in a water bath at 50°C with stirring for 4 h, cool to room temperature, and then slowly add the solution to the activation solution prepared in step A2. Stir the mixture at 400-600 rpm at 30-35°C for 6-12 h. After the reaction is completed, the product is obtained. The product is extracted with dichloromethane, and then placed in a rotary evaporator to evaporate the dichloromethane. After complete evaporation, urea / stearic acid conjugate is obtained.

[0026] This embodiment also provides a method for preparing macroporous alumina, which specifically comprises the following steps: S1. Weigh 100 mg of urea / stearic acid conjugate and add it to 10 mL of water. Stir until completely dissolved to obtain a surfactant solution. Weigh aluminum sulfate and add it to water. Dissolve evenly to prepare a 1 mol / L aluminum sulfate solution. S2, add 1.5 g potassium carbonate, 5 mL n-propanol, 10 mL ethyl acetate, 1.5 g sucrose and 95 mL water into a 150 mL container, stir and disperse evenly, continue to add the surfactant solution prepared in step S1, stir and disperse evenly, and obtain a mixed solution; S3, adding 40 mL of aluminum sulfate solution dropwise to the mixed solution prepared in step S2, stirring at 500 rpm for 4 h to form a uniform emulsion, adding 5 mL of triethylamine and 4 mL of triethoxysilane, stirring for 30 min, and standing for 8 h after the reaction is completed to obtain a sol solution; S4, placing the sol solution prepared in step S3 in an oven at 60° C. and drying for 5 h, then heating to 80° C. and drying until the sol solution is completely free of moisture to obtain a solid precursor; S5. Place the solid precursor obtained in step S4 in a muffle furnace, and heat it to 600°C at a heating rate of 8°C / min under the protection of a nitrogen flow at a flow rate of 1 L / min, and maintain it for 5 hours. After naturally cooling to room temperature, obtain the product, wash the product three times with water and ethanol alternately, and obtain macroporous alumina after drying.

[0027] Comparative Example 1: This comparative example proposes a macroporous alumina, which differs from Example 1 only in that potassium carbonate is not added, and the remaining components, component contents, and experimental steps are the same as those of Example 1.

[0028] Comparative Example 2: This comparative example proposes a macroporous alumina, which differs from Example 1 only in that ethyl acetate is not added, and the remaining components, component contents, and experimental steps are the same as those of Example 1.

[0029] Comparative Example 3: This comparative example proposes a macroporous alumina, which is different from Example 1 only in that urea is not added.

[0030] Comparative Example 4: This comparative example proposes a macroporous alumina, which is different from Example 1 only in that it is not modified with triethoxysilane.

[0031] Test Example 1: The microscopic morphology of the macroporous alumina prepared in Examples 1-3 of the present invention and Comparative Examples 1-3 was observed using a scanning electron microscope.

[0032] Figure 1 is a scanning electron microscope image of the macroporous alumina prepared in Example 1 of the present invention, Figure 2 is a scanning electron microscope image of the macroporous alumina prepared in Example 2 of the present invention, Figure 3 3 is a scanning electron microscope image of the macroporous alumina prepared in Example 3 of the present invention. As shown in the figure, the surfaces of the alumina prepared in Examples 1-3 are all distributed with significantly larger and uniform pores, with a diameter of about 1-2 μm, indicating that the macroporous alumina of the present invention was successfully prepared. Figure 4 is a scanning electron microscope image of the macroporous alumina prepared in Comparative Example 1 of the present invention, Figure 5 is a scanning electron microscope image of the macroporous alumina prepared in Comparative Example 2 of the present invention, Figure 6 This is a scanning electron microscope image of the macroporous alumina prepared in comparative example 3 of the present invention. As shown in the figure, the pore size of the alumina prepared in the comparative example is smaller than that in Example 1, and the void density is smaller, indicating that potassium carbonate, urea / carboxyl surfactant conjugate and ethyl acetate can effectively expand the pore size of the synthetic alumina.

[0033] Test Example 2: The specific surface area and structure of the macroporous alumina prepared in Example 1 were analyzed using BET test and XRD test.

[0034] Figure 7 This is the XRD diagram of the macroporous alumina prepared in Example 1 of the present invention. As shown in the figure, the macroporous alumina prepared in Example 1 has obvious X-ray diffraction peaks, a regular and orderly structure, and characteristic peaks that conform to the standard diffraction peaks of γ-alumina, indicating that the macroporous alumina described in the present invention is successfully prepared.

[0035] The specific surface areas of the macroporous aluminas prepared in Examples 1 to 3 and Comparative Examples 1 to 4 were analyzed by BET test and XRD test, and the results are shown in Table 1 below; Table 1. Specific surface area results of macroporous alumina prepared in Examples and Comparative Examples

[0036] Table 1 shows the specific surface area results of the macroporous alumina prepared in Examples 1 to 3 of the present invention and Comparative Examples 1 to 4, which show that the macroporous alumina has a relatively high specific surface area and is successfully prepared.

[0037] Catalytic reaction test: The macroporous alumina samples prepared in Example 1 of the present invention and Comparative Examples 1 to 4 were dried and pretreated at 100°C for 2h, 0.5g of the sample was added with 20mL of ethyl acetate and 40mL of water, the reaction temperature was maintained at 70°C, and the mixture was stirred evenly at 400rpm. The sample was sampled once every 30min, and the concentration change of ethyl acetate was detected by high performance liquid chromatography. The conversion rate was calculated as (initial concentration of ethyl acetate-residual concentration of ethyl acetate) / initial concentration of ethyl acetate × 100%, and the conversion rates at 30min, 60min and 120min were recorded. After the reaction, the catalyst sample was separated from the reaction system, washed three times with water and ethanol, and the catalyst was vacuum dried at 100°C again. The above reaction process was repeated for three cycles. The results are shown in Table 2.

[0038] Table 2. Results of macroporous alumina catalytic reactions

[0039] It can be seen from the results in Table 1 above that the macroporous alumina prepared by the present invention has excellent catalytic efficiency and can maintain good catalytic performance in multiple cycle tests; it can be seen from the results of Comparative Example 1 and Example 1 that potassium carbonate plays a role in releasing gas and expanding pores during high-temperature calcination. Lack of potassium carbonate will lead to smaller pore size, uneven pore structure, reduced specific surface area, lower catalytic efficiency, and due to poor stability, the conversion rate decreases significantly after multiple cycle tests; it can be seen from the results of Comparative Example 2 and Example 1 that due to the absence of ethyl acetate, the uniformity in the solution will be significantly improved, resulting in the inability to form a grid structure, thereby affecting the generation of pores, and the pore size finally formed is small and unevenly distributed, the active sites in the catalytic reaction are insufficiently exposed, the reaction efficiency and selectivity will decrease, and the uneven pore distribution causes the reaction efficiency to decrease during multiple cycles; it can be seen from the results of Comparative Example 3 and Example 1 that there is no The decomposition of urea produces gas, and the pore expansion is limited, resulting in a relatively small pore size and a decrease in porosity, which affects the specific surface area of ​​the catalyst and the diffusion channel of the reactants. The gas decomposed by urea and the gas decomposed by potassium carbonate act synergistically to form a macroporous structure through internal pressure. In the absence of urea, the synergistic effect fails, resulting in the inability to effectively expand the pore size, and the porosity and reaction efficiency are significantly reduced. It can be seen from the results of Comparative Example 4 and Example 1 that the triethoxysilane coating can effectively enhance the structural stability of the catalyst at high temperatures. The lack of this coating causes the catalyst surface to easily agglomerate at high temperatures. In addition, triethoxysilane and the pore structure of macroporous alumina act synergistically to improve the acid-base properties and surface stability of the catalyst. The lack of this synergistic effect leads to a decline in many aspects of the catalyst performance, especially the selectivity and stability in acid-base catalytic reactions are significantly reduced, and its service life and stability are significantly affected in multiple cycle tests.

[0040] The present invention and its implementation methods are described above, which is not restrictive. The drawings are only one of the implementation methods of the present invention, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it and design methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.

Claims

1. A macroporous alumina, It is characterized in that The macroporous alumina synthesis raw materials include the following components: potassium carbonate, ethyl acetate, low-carbon alcohol, urea / carboxyl surfactant coupling compound, aluminum salt, triethylamine, triethoxysilane, sucrose and water; The preparation method of the urea / carboxyl surfactant conjugate comprises the following steps: A1. Dissolve urea in anhydrous ethanol, stir until completely dissolved, add acetic anhydride and anhydrous pyridine, stir and react at room temperature for 2-4 hours. After the reaction is completed, pour the reaction mixture into an excess of 0°C ether solution, centrifuge, take the precipitate, wash with ether, and obtain acetylated urea; A2. Add the carboxyl surfactant to 100 mL of ethanol, stir to completely dissolve, continue to add EDC, stir at 500 rpm for 3 h, and after the reaction is completed, continue to add NHS, stir at 500 rpm for 3 h to obtain an activated solution; A3. Dissolve the acetylated urea prepared in step A1 in 100 mL of deionized water, heat in a water bath at 50°C with stirring for 24 h, cool to room temperature, and then slowly add the solution to the activation solution prepared in step A2. Stir the mixture at 400-600 rpm at 30-35°C for 6-12 h. After the reaction is completed, the product is obtained. The product is extracted with dichloromethane, and then placed in a rotary evaporator to evaporate the dichloromethane. After complete evaporation, a urea / carboxyl surfactant conjugate is obtained.

2. The macroporous alumina according to claim 1, It is characterized in that The ratio of urea, anhydrous ethanol, acetic anhydride and anhydrous pyridine used in step A1 is 0.1 mol: 100 mL: 0.12 mol: 0.6 mL; the ratio of carboxyl surfactant, ethanol, EDC and NHS used in step A2 is 0.1 mol: 100 mL: 0.11 mol: 0.11 mol.

3. A macroporous alumina according to claim 2, It is characterized in that The carboxyl surfactant in step A2 is any one of stearic acid, oleic acid, palmitic acid, capric acid and sodium laurate.

4. A macroporous alumina according to claim 3, It is characterized in that The low-carbon alcohol is any one of methanol, ethanol, n-propanol and isopropanol.

5. A macroporous alumina according to claim 4, It is characterized in that The aluminum salt is any one of aluminum chloride, aluminum nitrate and aluminum sulfate.

6. A method for preparing the macroporous alumina according to any one of claims 1 to 5, It is characterized in that The specific steps include: S1, weighing urea / carboxyl surfactant conjugate, adding it to water, stirring until completely dissolved to obtain a surfactant solution, weighing aluminum salt, adding it to water, and dissolving it evenly to obtain an aluminum salt solution; S2, adding potassium carbonate, low-carbon alcohol, ethyl acetate, sucrose and water into a container, stirring and dispersing them evenly, and continuing to add the surfactant solution prepared in step S1, stirring and dispersing them evenly to obtain a mixed solution; S3, adding aluminum salt solution dropwise to the mixed solution prepared in step S2, stirring for 3-6 h to form a uniform emulsion, continuing to add triethylamine and triethoxysilane, continuing to stir for 30-60 min, and standing for 6-12 h after the reaction is completed to obtain a sol solution; S4, drying the sol solution prepared in step S3 at 60° C. for 4-6 h, and then heating to 80° C. for drying until the sol solution is completely free of water to obtain a solid precursor; S5. The solid precursor obtained in step S4 is heated to 500-700°C at a heating rate of 5-10°C / min under the protection of a nitrogen flow, maintained for 3-5 hours, and naturally cooled to room temperature to obtain a product, which is then washed and dried to obtain macroporous alumina.

Citation Information

Patent Citations

  • Method for preparing porous spherical high-purity alumina powder

    CN104843753A

  • Method for preparing alumina carrier with large pore volume

    CN106747591A

  • Macroporous alumina and preparation method thereof

    CN110467206A

  • Macroporous alumina and preparation method thereof

    CN110935429A

  • Silicon-modified macroporous alumina and preparation method thereof

    CN110935433A

Cited By

  • Lattice oxygen-driven electronegativity enhanced multi-center ozone catalyst for treating wastewater as well as preparation method and application of lattice oxygen-driven electronegativity enhanced multi-center ozone catalyst

    CN119793445A

  • Preparation method of lightweight high-strength composite board

    CN120080616A

  • Preparation method of high-pore-volume theta-aluminum oxide

    CN120383329A