Preparation method of high-purity bisphenol F

By using liquid acid catalysts and multi-stage separation and purification processes, the side reactions and impurities in the preparation of high-purity bisphenol F were solved, achieving high-yield and high-purity bisphenol F production, which is suitable for chip-grade high-purity epoxy resins.

CN119019227APending Publication Date: 2024-11-26HUNAN BINSHENG NEW MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411121719.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing technologies are difficult to efficiently prepare high-purity bisphenol F, and suffer from problems such as numerous side reactions, easy catalyst deactivation, low product yield, and high impurity content, which especially affects product quality in the application of chip-grade high-purity epoxy resin.

Method used

High-purity bisphenol F was obtained through a homogeneous catalytic reaction using a liquid acid catalyst, combined with a three-stage separation, extraction, phenol removal, and three-stage crystallization process, including a first-stage cooling crystallization, a second-stage cooling crystallization, and a third-stage cooling crystallization.

Benefits of technology

It improved the yield and purity of bisphenol F, reduced the content of oligomers and impurities, met the requirements of chip-grade high-purity epoxy resin, and enhanced the added value and competitiveness of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a preparation method of high-purity bisphenol F. The preparation method specifically comprises the following steps: (1) a reaction section; (2) a liquid separation section; (3) extraction section; (4) a third-stage dephenolization section; (5) tertiary crystallization section; and (6) filtering and drying. The first-grade high-purity bisphenol F product prepared by the invention can be applied to chip-grade and electronic-grade high-end resin materials, the second-grade high-purity bisphenol F product can be applied to electronic-grade medium-and-high-end resin materials and wind power-grade resin materials, and the third-grade high-purity bisphenol F product can be applied to other medium-and-low-end low-viscosity resin materials. The problems in current chip semiconductors and advanced composite materials are solved, meanwhile, a large amount of low-viscosity special resin is provided for the traditional industry, and the added value and competitiveness of products are greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of resin synthesis, and more particularly to a method for preparing high-purity bisphenol F. Background Art

[0002] Bisphenol F (BPF) monomer is synthesized by acid-catalyzed reaction of phenol and formaldehyde under high phenol-formaldehyde ratio conditions. It contains three isomers: para-position (4,4'-bisphenol F isomer), ortho-para-position (2,4'-bisphenol F isomer) and ortho-ortho-position (2,2'-bisphenol F isomer). High-purity bisphenol F monomer will be further used to prepare high-purity bisphenol F epoxy resin.

[0003] With the development of advanced chip packaging technology, chip-level high-purity bisphenol F epoxy resin is required to be colorless and transparent, with low viscosity, low total chlorine, and epoxy equivalent close to the theoretical value. However, residual phenol in bisphenol F products can easily cause discoloration of bisphenol F and its epoxy resin, and at the same time have an adverse effect on the epoxy equivalent of downstream chip-level high-purity epoxy resin. Oligomers will have an adverse effect on the low viscosity of high-purity epoxy resin.

[0004] At present, from the perspective of industrial large-scale production, the shortcomings of the above high-purity and low-viscosity problems are solved mainly from the three key process flows of reaction section, phenol removal section and refining section:

[0005] 1. Reaction Section

[0006] (1) Oxalic acid method: Phenol is distilled and thermally decomposed to remove the catalyst, and the production process is simple; however, there are many side reactions, the para-BPF content is low (20%-30%), there are many oligomers, and the overall yield of bisphenol F monomer is low.

[0007] (2) Solid acid method: The catalyst and product can be easily separated; however, the bisphenol F oligomer by-product can easily clog the catalyst pores, causing the catalyst to fail easily, making replacement difficult and industrial scale-up production difficult. There have been no reports of industrial production of bisphenol F prepared by solid acid catalysis, but there are many solid acid catalytic synthesis techniques for bisphenol F in academic literature.

[0008] (3) Liquid inorganic acid method: For medium-strong acid phosphoric acid, there are few side reactions, high para-BPF content, and high overall yield of bisphenol F; however, there are problems such as the recovery and utilization of acid catalysts, removal of residual catalysts, recycling of water, and a longer production process.

[0009] 2. Dephenolization Section

[0010] (1) Normal temperature distillation tower: large evaporation processing capacity and simple equipment; but high evaporation temperature, long residence time, prone to side reactions; incomplete phenol distillation, high phenol impurity content.

[0011] (2) Vacuum distillation tower: large evaporation processing capacity and simple equipment; however, phenol distillation is incomplete and the phenol impurity content is high.

[0012] (3) Short-path scraped film distiller: high distillation efficiency and low phenol impurity content; but the equipment structure is complex and the equipment vacuum degree requirement is high.

[0013] 3. Refining Section

[0014] Recrystallization method: The equipment and process are simple; however, the isomers are not separated and the products cannot be graded.

[0015] Therefore, how to develop a novel method for preparing high-purity bisphenol F is an urgent problem to be solved by those skilled in the art. Summary of the invention

[0016] In view of this, the object of the present invention is to provide a method for preparing high-purity bisphenol F to solve the deficiencies in the prior art.

[0017] In order to achieve the above object, the present invention adopts the following technical solution:

[0018] A method for preparing high-purity bisphenol F specifically comprises the following steps:

[0019] (1) Reaction Section

[0020] Heat phenol until it is completely melted, add a liquid acid catalyst, stir until the mixture is uniformly mixed, dropwise add formaldehyde solution, react, and obtain a crude reaction product solution;

[0021] (2) Liquid separation section

[0022] The crude reaction product solution is allowed to stand for stratification, separated, and washed with water to obtain an upper reaction product oil phase and a lower catalyst water phase;

[0023] (3) Extraction Section

[0024] The upper reaction product oil phase is washed with water and extracted to obtain an extraction phase containing the reaction product and a raffinate phase containing water and the catalyst respectively;

[0025] (4) Three-stage dephenolization section

[0026] The extract phase containing the reaction product is subjected to three-stage dephenolization, wherein the first stage is dehydration / toluene / phenol mixture, the second stage is dephenolization, and the third stage is scraped film distillation to remove residual phenol to obtain a dephenolization reaction product;

[0027] (5) Three-stage crystallization section

[0028] The dephenolization reaction product is subjected to three-stage crystallization, first-stage cooling crystallization, and first-stage centrifugal filtration to obtain a high-purity bisphenol F product I and a filtrate I, respectively; the high-purity bisphenol F product I is subjected to a first-stage drying to obtain a first-stage high-purity bisphenol F product;

[0029] The filtrate I is subjected to second-stage cooling crystallization and second-stage centrifugal filtration to obtain high-purity bisphenol F product II and filtrate II, respectively; the high-purity bisphenol F product II is subjected to second-stage drying to obtain a secondary high-purity bisphenol F product;

[0030] The filtrate II is subjected to third-stage cooling crystallization and third-stage centrifugal filtration to obtain high-purity bisphenol F product III and filtrate III respectively; the high-purity bisphenol F product III is subjected to third-stage drying to obtain a third-grade high-purity bisphenol F product.

[0031] Furthermore, in the above step (1), the liquid acid catalyst is at least one of a liquid organic acid, a liquid inorganic acid, a liquid acidic ionic liquid and a liquid acidic salt solution, preferably liquid phosphoric acid; the mass ratio of phenol to the liquid acid catalyst is (6-14):1; the mass ratio of phenol to the formaldehyde solution is (4-12):1; the mass fraction of the formaldehyde solution is 37%, and the dropwise addition time is 0.5-2h; the reaction temperature is 50-75°C, and the reaction time is 1-5h.

[0032] The above further beneficial effect is that in the reaction section, the present invention adopts the phosphoric acid method. Compared with the oxalic acid method, the present invention has fewer side reactions, higher para-BPF content, less oligomers, and higher overall yield of bisphenol F monomer. Compared with the solid acid method, the catalyst of the present invention has good reusability. Compared with the liquid inorganic acid method, the present invention is more suitable for producing high para-bisphenol F content and high bisphenol F yield.

[0033] After the reaction, the formaldehyde conversion rate in the crude reaction product solution is 99% to 100%, the selectivity of bisphenol F is 95% to 99.5%, the content of 4,4'-bisphenol F isomer is 40% to 50%, the content of 2,4'-bisphenol F isomer is 35% to 45%, and the content of 2,2'-bisphenol F isomer is 10% to 15%.

[0034] Furthermore, in the above step (2), the water washing temperature is 50-80° C., the solution is pure water, the amount used is 1-3 times the volume of the crude reaction product oil phase, and the number of times is 1-3 times.

[0035] Furthermore, in the above step (3), the extraction temperature is 25-85°C, the extraction agent is a toluene / water mixture, and the amount used is 0.3-3 times the volume of the upper reaction product oil phase; in the toluene / water mixture, the mass of toluene and water is (1-3):1.

[0036] A further beneficial effect of the above method is that after extraction, the concentration of phosphoric acid in the extraction phase containing the reaction product is 1-100 ppm.

[0037] Furthermore, in the above step (4), the temperature of the first stage dehydration / toluene / phenol mixture is 70-110°C and the pressure is 50-150 mbar; the temperature of the second stage dephenolization is 150-180°C and the pressure is 20-50 mbar; the temperature of the third stage scraped film distillation for removing residual phenol is 150-180°C and the pressure is 20-50 mbar.

[0038] The further beneficial effect of adopting the above method is that in the dephenolization process, the present invention adopts a three-stage continuous dephenolization system. The first stage rising film evaporation of toluene and phenol mixture can solve the problem of large phenol distillation amount; the second stage falling film evaporation of phenol can solve the problem of removing a large amount of phenol; the third stage scraping film stripping evaporation of residual phenol can solve the problem of removing residual phenol. Continuous operation can ensure large processing capacity and stable production.

[0039] After three-stage dephenolization, the content of phenol in the dephenolization reaction product is 0.001% to 0.1%.

[0040] Furthermore, in the above step (5), the solvent concentration of the first stage cooling crystallization is 50% to 80%, the cooling rate is 5 to 20°C / min, and the temperature is 70 to 90°C; the solvent concentration of the second stage cooling crystallization is 30% to 60%, and the temperature is 5 to 50°C; the solvent concentration of the third stage cooling crystallization is 20% to 40%, and the temperature is 10 to 30°C.

[0041] The further beneficial effect of adopting the above method is that in the refining section, the present invention adopts a three-stage crystallization method. The first stage: thermal insulation rapid crystallization to obtain a high-purity product of para-bisphenol F. After drying, the content of 4,4'-bisphenol F isomers in the first-stage high-purity bisphenol F product is 90% to 99.5%; the second stage: concentration-cooling crystallization to obtain a high-purity product of ortho-bisphenol F. After drying, the content of 2,4'-bisphenol F isomers in the second-stage high-purity bisphenol F product is 50% to 70%; the third stage: concentration-cooling crystallization to obtain a high-purity bisphenol F product. After drying, the content of 2,2'-bisphenol F isomers in the third-stage high-purity bisphenol F product is 50% to 80%.

[0042] Finally, the total yield of bisphenol F in the high-purity bisphenol F finished product is 90% to 99%, the purity of bisphenol F is 99% to 99.9%, and the content of oligomers is less than 0.1% to 1%.

[0043] Furthermore, the method for preparing high-purity bisphenol F further comprises step (6) a catalyst recovery section: distilling the lower catalyst aqueous phase of the liquid separation section of step (2) and the residual phase containing water and catalyst of the extraction section of step (3), and using the recovered catalyst for reaction in the reaction section of step (1), and using the recovered pure water for water washing in the liquid separation section of step (2).

[0044] A further beneficial effect of the above method is that after recovery, the recovery rate of the catalyst is 99% to 100%.

[0045] Furthermore, the method for preparing high-purity bisphenol F further comprises a step (7) solvent recovery section: the water / toluene recovered in the tertiary dephenolization section in step (4) is used in the extraction section in step (3) as an extractant for extraction, and the recovered phenol is used in the reaction section in step (1) as a raw material for reaction; and the solvent recovered in the tertiary crystallization section in step (5) is used in the first stage cooling crystallization as a crystallization solvent for crystallization.

[0046] A further beneficial effect of the above method is that after recovery, the recovery rate of the solvent is 99% to 100%.

[0047] It can be seen from the above technical solution that compared with the prior art, the beneficial effects of the present invention are as follows:

[0048] 1. In terms of reaction, the present invention adopts homogeneous catalysis of liquid acid and medium-strong acid catalyst for catalytic reaction, the yield of bisphenol F product is high, and the content of 4,4'-bisphenol F isomer is high (40% to 45%); phenol is added first and then acid is added during the reaction, which is conducive to the co-feeding of the recovered acid-containing phenol raw material and the phenolic acid catalyst, thereby simplifying the production process.

[0049] 2. In terms of separation, the present invention recycles a large amount of low-phenol content acid catalysts through a simple liquid separation process, which is beneficial to saving energy consumption; the residual catalyst in the crude reaction product adopts an integrated process of multi-stage water washing and extraction to ensure that the residual content of the acid catalyst reaches the ppm level, which is beneficial to reducing the occurrence of side reactions in the subsequent high-temperature distillation process; the three-stage dephenolization process performs graded distillation and graded condensation according to the differences in boiling points and contents of solvents and unreacted raw materials, which is beneficial to energy saving and consumption reduction. At the same time, the last stage of scraped film distillation removes residual phenol to ensure that the phenol impurity content does not affect subsequent crystallization, which is beneficial to improving the high purity requirements of the product.

[0050] 3. In terms of crystallization and purification, fractional crystallization is carried out according to the requirements of different isomer contents of the product to obtain high-purity products with different isomer contents. The products have good appearance, high purity, granular form, and are easy to package and apply downstream.

[0051] 4. In terms of product quality and downstream applications, the first-level high-purity bisphenol F products can be used in chip-level and electronic-grade high-end resin materials, the second-level high-purity bisphenol F products can be used in electronic-grade mid-to-high-end resin materials and wind power-grade resin materials, and the third-level high-purity bisphenol F products can be used in other mid-to-low-end low-viscosity resin materials, which will help solve the current problems in chip semiconductors and advanced composite materials, and at the same time provide a large number of low-viscosity specialty resins for traditional industries, greatly improving the added value and competitiveness of the products. DETAILED DESCRIPTION

[0052] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0053] Example 1

[0054] The preparation method of high-purity bisphenol F specifically comprises the following steps:

[0055] (1) Reaction Section

[0056] Add phenol to the reaction kettle, heat until completely melted, add liquid phosphoric acid catalyst, stir until well mixed, dropwise add 37% formaldehyde solution within 1.5 hours, react at 65°C for 3 hours to obtain a crude reaction product solution;

[0057] Wherein, the mass ratio of phenol to liquid phosphoric acid catalyst is 10:1, and the mass ratio of phenol to formaldehyde solution is 10:1;

[0058] (2) Liquid separation section

[0059] The crude reaction product solution was allowed to stand for stratification, and then washed with pure water for 3 times at 65°C, with the amount of pure water being 3 times the volume of the crude reaction product oil phase, to obtain an upper reaction product oil phase and a lower catalyst water phase, respectively;

[0060] (3) Extraction Section

[0061] The upper reaction product oil phase is washed and extracted with a toluene / water mixture at 65°C, wherein the amount of the toluene / water mixture is 3 times the volume of the upper reaction product oil phase, to obtain an extraction phase containing the reaction product and a raffinate phase containing water and the catalyst, respectively;

[0062] Wherein, the mass ratio of toluene to water in the toluene / water mixture is 1:1;

[0063] (4) Three-stage dephenolization section

[0064] The extract phase containing the reaction product is subjected to three-stage dephenolization, wherein the first stage is dephenolization of a water / toluene / phenol mixture at a temperature of 100°C and a pressure of 100 mbar; the second stage is dephenolization at a temperature of 160°C and a pressure of 30 mbar; the third stage is dephenolization of residual phenol at a temperature of 160°C and a pressure of 20 mbar to obtain a dephenolization reaction product;

[0065] (5) Three-stage crystallization section

[0066] The dephenolization reaction product is subjected to three-stage crystallization, wherein the first stage is cooling crystallization, the solvent concentration is 50%, the cooling rate is 20°C / min, the temperature is 90°C, and the first stage is centrifugal filtration to obtain a high-purity bisphenol F product I and a filtrate I respectively; the high-purity bisphenol F product I is subjected to the first stage drying to obtain a first-stage high-purity bisphenol F product;

[0067] The filtrate I is subjected to a second stage of cooling crystallization, with a solvent concentration of 40% and a temperature of 30° C., and a second stage of centrifugal filtration to obtain a high-purity bisphenol F product II and a filtrate II, respectively; the high-purity bisphenol F product II is subjected to a second stage of drying to obtain a secondary high-purity bisphenol F product;

[0068] The filtrate II is subjected to third-stage cooling crystallization, with a solvent concentration of 40% and a temperature of 10°C, and is subjected to third-stage centrifugal filtration to obtain high-purity bisphenol F product III and filtrate III, respectively; the high-purity bisphenol F product III is subjected to third-stage drying to obtain a third-grade high-purity bisphenol F product;

[0069] (6) Catalyst recovery section

[0070] The lower catalyst aqueous phase of the liquid separation section of step (2) and the residual phase containing water and catalyst of the extraction section of step (3) are distilled, the recovered catalyst is used for reaction in the reaction section of step (1), and the recovered pure water is used for water washing in the liquid separation section of step (2);

[0071] (7) Solvent recovery section

[0072] The water / toluene recovered from the tertiary dephenolization section of step (4) is used as an extractant in the extraction section of step (3) for extraction, and the recovered phenol is used as a raw material in the reaction section of step (1) for reaction; the solvent recovered from the tertiary crystallization section of step (5) is used as a crystallization solvent in the first stage cooling crystallization for crystallization.

[0073] Example 2

[0074] The only difference from Example 1 is that in the reaction section of step (1), the reaction temperature is 50°C.

[0075] Example 3

[0076] The only difference from Example 1 is that in the reaction section of step (1), the reaction temperature is 55°C.

[0077] Example 4

[0078] The only difference from Example 1 is that in the reaction section of step (1), the reaction temperature is 60°C.

[0079] Example 5

[0080] The only difference from Example 1 is that in the reaction section of step (1), the reaction temperature is 70°C.

[0081] Example 6

[0082] The only difference from Example 1 is that in the reaction section of step (1), the reaction temperature is 75°C.

[0083] Example 7

[0084] The only difference from Example 1 is that in the reaction section of step (1), the reaction time is 1 h.

[0085] Example 8

[0086] The only difference from Example 1 is that in the reaction section of step (1), the reaction time is 2 h.

[0087] Example 9

[0088] The only difference from Example 1 is that in the reaction section of step (1), the reaction time is 4 hours.

[0089] Example 10

[0090] The only difference from Example 1 is that in the reaction section of step (1), the reaction time is 5 h.

[0091] Embodiment 11

[0092] The only difference from Example 1 is that in the reaction section of step (1), the mass ratio of phenol to formaldehyde solution is 4:1.

[0093] Example 12

[0094] The only difference from Example 1 is that in the reaction section of step (1), the mass ratio of phenol to formaldehyde solution is 6:1.

[0095] Example 13

[0096] The only difference from Example 1 is that in the reaction section of step (1), the mass ratio of phenol to formaldehyde solution is 7:1.

[0097] Embodiment 14

[0098] The only difference from Example 1 is that in the reaction section of step (1), the mass ratio of phenol to formaldehyde solution is 8:1.

[0099] Embodiment 15

[0100] The only difference from Example 1 is that in the reaction section of step (1), the mass ratio of phenol to formaldehyde solution is 9:1.

[0101] Example 16

[0102] The only difference from Example 1 is that in the reaction section of step (1), the mass ratio of phenol to formaldehyde solution is 12:1.

[0103] Embodiment 17

[0104] The only difference from Example 1 is that in the reaction section of step (1), the mass ratio of phenol to liquid phosphoric acid catalyst is 6:1.

[0105] Embodiment 18

[0106] The only difference from Example 1 is that in the reaction section of step (1), the mass ratio of phenol to liquid phosphoric acid catalyst is 8:1.

[0107] Embodiment 19

[0108] The only difference from Example 1 is that in the reaction section of step (1), the mass ratio of phenol to liquid phosphoric acid catalyst is 12:1.

[0109] Embodiment 20

[0110] The only difference from Example 1 is that in the reaction section of step (1), the mass ratio of phenol to liquid phosphoric acid catalyst is 14:1.

[0111] Comparative Example 1

[0112] The oxalic acid method is used, and the only difference from Example 1 is that in the reaction section of step (1), the catalyst is oxalic acid.

[0113] Comparative Example 2

[0114] The solid acid method is used, and the only difference from Example 1 is that in the reaction section of step (1), the catalyst is an acidic ion exchange resin.

[0115] Comparative Example 3

[0116] The only difference from Example 1 is that step (4) adopts a secondary dephenolization section, specifically:

[0117] The extract phase containing the reaction product is subjected to two-stage dephenolization, wherein the first stage is dephenolization of a water / toluene / phenol mixture at a temperature of 100° C. and a pressure of 100 mbar; the second stage is dephenolization at a temperature of 160° C. and a pressure of 30 mbar to obtain a dephenolization reaction product.

[0118] Comparative Example 4

[0119] The only difference from Example 1 is that step (5) adopts a primary crystallization section, specifically:

[0120] The dephenolization reaction product is dissolved in toluene solvent for crystallization at a solvent concentration of 40% and a temperature of 20° C. to obtain a high-purity bisphenol F product.

[0121] Comparative Example 5

[0122] The only difference from Example 4 is that the temperature is 30°C.

[0123] Comparative Example 6

[0124] The only difference from Example 4 is that the temperature is 40°C.

[0125] Performance Testing

[0126] 1. Reaction section

[0127] The dephenolization reaction products obtained in the dephenolization process of step (4) of Example 1-20 and Comparative Example 1-2 were respectively taken to detect the bisphenol F yield and the 4,4'-bisphenol F isomer content.

[0128] Wherein, the yield of bisphenol F = the actual amount of three isomers of bisphenol F / the theoretical amount of bisphenol F completely converted from formaldehyde × 100%;

[0129] The content of 4,4'-bisphenol F isomers was measured by high performance liquid chromatography.

[0130] The results are shown in Table 1.

[0131] Table 1 Bisphenol F yield and 4,4'-bisphenol F isomer content of dephenolization reaction products of Examples 1-20 and Comparative Examples 1-2

[0132]

[0133]

[0134] As shown in Table 1, the phosphoric acid catalyst used in the present invention has a higher bisphenol F yield and 4,4'-bisphenol F isomer content compared with the oxalic acid catalyst of Comparative Example 1. Compared with the acidic ion exchange resin solid catalyst of Comparative Example 2, the phosphoric acid catalyst used in the present invention has a higher bisphenol F yield.

[0135] In addition, in the reaction section of the present invention, the reaction temperature, reaction time, phenol-formaldehyde ratio and phenol-acid ratio all have an effect on the bisphenol F yield and the 4,4'-bisphenol F isomer content. Under the conditions of reaction temperature of 65° C., phenol-formaldehyde ratio of 10:1, phenol-acid ratio of 10:1 and reaction time of 3 h, a synergistic effect is achieved, the bisphenol F yield reaches 93.8%, and the 4,4'-bisphenol F isomer content reaches 43.6%.

[0136] 2. Liquid separation section

[0137] The lower catalyst aqueous phase (phosphoric acid solution) of the liquid separation stage in step (2) of Example 1 was taken to determine the phosphoric acid concentration and calculate the phosphoric acid recovery rate. The experiment was repeated four times in parallel.

[0138] The phosphoric acid concentration was analyzed by volumetric method, using thymolphthalein as indicator solution, removing phenol, and titrating phosphoric acid with 0.5 mol / L sodium hydroxide standard titration solution to determine the phosphoric acid concentration;

[0139] Phosphoric acid recovery rate = mass of phosphoric acid separated and recovered / total mass of phosphoric acid input × 100%.

[0140] The results are shown in Table 2.

[0141] Table 2 Phosphoric acid concentration and phosphoric acid recovery rate of the lower catalyst aqueous phase of Example 1

[0142] Number of trials Static temperature / ℃ Phosphoric acid concentration / % Phosphoric acid recovery rate / % 1 65 69.1 82.1 2 65 69.2 83.5 3 65 72.4 85.4 4 65 69.3 81.6

[0143] As shown in Table 2, under the reaction temperature, the phosphoric acid concentration and phosphoric acid recovery rate of the four parallel experiments were relatively stable, and most of the phosphoric acid could be directly recovered by liquid separation.

[0144] 3. Extraction section

[0145] The raffinate phase (phosphoric acid solution) containing water and catalyst in the extraction stage of step (3) of Example 1 was taken, the phosphoric acid concentration was determined and the phosphoric acid recovery rate was calculated, and the type of extractant and the extraction temperature were changed for comparison.

[0146] The results are shown in Table 3.

[0147] Table 3 Phosphoric acid concentration and phosphoric acid recovery rate of the raffinate phase containing water and catalyst in Example 1

[0148] Extraction agent Temperature / ℃ Extractant content / % Water content / % Phosphoric acid recovery rate / % none 65 30 30 34.8 Cyclohexane 65 30 30 66.6 Ethyl acetate 65 30 30 72.6 Toluene 25 30 30 65.9 Toluene 45 30 30 75.6 Toluene 65 30 30 81.3 Toluene 70 30 30 83.6 Toluene 80 30 30 78.7

[0149] As shown in Table 3, the difference in solubility of phosphoric acid in different extractants leads to great differences in the recovery rate of phosphoric acid. Among them, toluene has the best extraction effect and the highest phosphoric acid recovery rate. The use of multi-stage extraction is beneficial to improving the total recovery rate of phosphoric acid and reducing the residual content of phosphoric acid.

[0150] 4. Dephenolization section

[0151] Take the reaction products after each stage of dephenolization in the three-stage dephenolization section in step (4) of Example 1, the dephenolization reaction product obtained in the two-stage dephenolization section in step (4) of Comparative Example 3, and the high-purity bisphenol F finished product obtained in the three-stage crystallization section in step (5) of Comparative Example 3, and calculate their residual phenol contents respectively.

[0152] Among them, the residual phenol content was determined by liquid chromatography.

[0153] The results are shown in Table 4.

[0154] Table 4 Residual phenol content in the dephenolization reaction products of Example 1 and Comparative Example 3

[0155]

[0156] As shown in Table 4, in Comparative Example 3, the residual phenol content reached 5% by using the vacuum distillation technology, and the residual phenol content in the high-purity bisphenol F product of the subsequent crystallization stage exceeded 0.3%. However, the present invention adopts a three-stage phenol distillation technology, in which the last stage adopts scraped film distillation, and the residual phenol content in the dephenolization reaction product can be reduced to 0.005%, and the residual phenol is basically not detected in the high-purity bisphenol F product of the subsequent crystallization stage.

[0157] 5. Crystallization section

[0158] The products after each stage of crystallization in the tertiary crystallization section of step (5) of Example 1 and the high-purity bisphenol F products obtained in the primary crystallization section of step (5) of Comparative Examples 4-6 were taken, and their bisphenol F yields and isomer (4,4'-bisphenol F isomer, 2,4'-bisphenol F isomer and 2,2'-bisphenol F isomer) contents were calculated respectively, and the crystallization temperature and solvent concentration were adjusted for comparison.

[0159] Wherein, the yield of bisphenol F = the mass of bisphenol F after crystallization and drying / the mass of bisphenol F in the mother liquor before crystallization;

[0160] The contents of three bisphenol F isomers were determined by area normalization method.

[0161] The results are shown in Table 5.

[0162] Table 5 Bisphenol F yield and isomer content of the crystalline products of Example 1 and Comparative Examples 4-6

[0163]

[0164] As shown in Table 5, the overall yield of bisphenol F in Comparative Examples 4-6 using a single crystallization technology is relatively low. The present invention uses a three-stage crystallization technology, in which the first stage of high-temperature crystallization is conducive to increasing the content of 4,4'-bisphenol F isomers and improving the added value of the product; the second stage of medium-temperature crystallization is conducive to increasing the yield of bisphenol F; and the third stage of low-temperature crystallization is conducive to further increasing the overall yield of bisphenol F products.

[0165] 6. Catalyst recovery section

[0166] It was measured that in the catalyst recovery section of step (6) of Example 1, the contents of phosphoric acid, water and phenol in the distilled product were 85%, 12% and 3% respectively, and the total recovery rate of phosphoric acid was 99.2%.

[0167] 7. Solvent recovery section

[0168] It was measured that the total recovery rate of the solvent in the solvent recovery section of step (7) of Example 1 was 99.5%.

[0169] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing high-purity bisphenol F, characterized in that: The specific steps include: (1) Reaction Section Heat phenol until it is completely melted, add a liquid acid catalyst, stir until the mixture is uniformly mixed, dropwise add formaldehyde solution, react, and obtain a crude reaction product solution; (2) Liquid separation section The crude reaction product solution is allowed to stand for stratification, separated, and washed with water to obtain an upper reaction product oil phase and a lower catalyst water phase; (3) Extraction Section The upper reaction product oil phase is washed with water and extracted to obtain an extraction phase containing the reaction product and a raffinate phase containing water and the catalyst respectively; (4) Three-stage dephenolization section The extract phase containing the reaction product is subjected to three-stage dephenolization, wherein the first stage is dehydration / toluene / phenol mixture, the second stage is dephenolization, and the third stage is scraped film distillation to remove residual phenol to obtain a dephenolization reaction product; (5) Three-stage crystallization section The dephenolization reaction product is subjected to three-stage crystallization, first-stage cooling crystallization, and first-stage centrifugal filtration to obtain a high-purity bisphenol F product I and a filtrate I, respectively; the high-purity bisphenol F product I is subjected to a first-stage drying to obtain a first-stage high-purity bisphenol F product; The filtrate I is subjected to second-stage cooling crystallization and second-stage centrifugal filtration to obtain high-purity bisphenol F product II and filtrate II, respectively; the high-purity bisphenol F product II is subjected to second-stage drying to obtain a secondary high-purity bisphenol F product; The filtrate II is subjected to third-stage cooling crystallization and third-stage centrifugal filtration to obtain high-purity bisphenol F product III and filtrate III respectively; the high-purity bisphenol F product III is subjected to third-stage drying to obtain a third-grade high-purity bisphenol F product.

2. The method for preparing high-purity bisphenol F according to claim 1, characterized in that: In step (1), the liquid acid catalyst is at least one of a liquid organic acid, a liquid inorganic acid, a liquid acidic ionic liquid and a liquid acidic salt solution; the mass ratio of the phenol to the liquid acid catalyst is (6-14):1; the mass ratio of the phenol to the formaldehyde solution is (4-12):1; the mass fraction of the formaldehyde solution is 37%, and the dropwise addition time is 0.5-2h; the reaction temperature is 50-75°C, and the reaction time is 1-5h.

3. The method for preparing high-purity bisphenol F according to claim 1, characterized in that: In step (2), the water washing temperature is 50-80° C., the solution is pure water, the amount used is 1-3 times the volume of the crude reaction product oil phase, and the number of times is 1-3 times.

4. The method for preparing high-purity bisphenol F according to claim 1, characterized in that: In step (3), the extraction temperature is 25-85° C., the extractant is a toluene / water mixture, and the amount used is 0.3-3 times the volume of the upper reaction product oil phase; in the toluene / water mixture, the mass of toluene and water is (1-3):

1.

5. The method for preparing high-purity bisphenol F according to claim 1, characterized in that: In step (4), the temperature of the first stage dehydration / toluene / phenol mixture is 70-110°C and the pressure is 50-150 mbar; the temperature of the second stage dephenolization is 150-180°C and the pressure is 20-50 mbar; the temperature of the third stage scraped film distillation for removing residual phenol is 150-180°C and the pressure is 20-50 mbar.

6. The method for preparing high-purity bisphenol F according to claim 1, characterized in that: In step (5), the solvent concentration of the first stage cooling crystallization is 50% to 80%, the cooling rate is 5 to 20°C / min, and the temperature is 70 to 90°C; the solvent concentration of the second stage cooling crystallization is 30% to 60%, and the temperature is 5 to 50°C; the solvent concentration of the third stage cooling crystallization is 20% to 40%, and the temperature is 10 to 30°C.

7. The method for preparing high-purity bisphenol F according to claim 1, characterized in that: The method further comprises step (6) a catalyst recovery section: distilling the lower catalyst aqueous phase of the liquid separation section of step (2) and the residual phase containing water and catalyst of the extraction section of step (3), using the recovered catalyst for reaction in the reaction section of step (1), and using the recovered pure water for water washing in the liquid separation section of step (2).

8. The method for preparing high-purity bisphenol F according to claim 1, characterized in that: The method further comprises a step (7) of solvent recovery: using the water / toluene recovered in the tertiary dephenolization section in the step (4) as an extractant in the extraction section in the step (3) for extraction, and using the recovered phenol in the reaction section in the step (1) as a raw material for reaction; and using the solvent recovered in the tertiary crystallization section in the step (5) as a crystallization solvent in the first stage of cooling crystallization for crystallization.