Preparation method of high-insulating-property epoxy insulating material based on fluorinated diluent modification
By modifying the epoxy resin system by fluorinated diluent, the problem of the resistivity of epoxy insulating materials decreasing when increasing the space charge migration rate is solved, and high insulation performance and good space charge migration ability are improved.
Patent Information
- Application Number
- CN202411130958.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-26
AI Technical Summary
When existing epoxy insulating materials increase the space charge migration rate, they often lead to a decrease in resistivity, affecting the insulation performance, and it is difficult to improve the insulation performance and space charge migration capability at the same time.
The epoxy resin system is modified by fluorinated diluents, and molecular orbital hybridization is achieved by replacing modified butylglycidyl ether (BGE) by fluorine atoms, improving the insulation performance and space charge migration ability of epoxy insulating materials.
The insulation strength and space charge migration ability of epoxy insulating materials are improved, while maintaining a high resistivity and avoiding space electric field distortion.
Smart Images

Figure CN119019815A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrical insulating materials, and in particular relates to a method for preparing a high-insulating performance epoxy insulating material modified by a fluorinated diluent. Background Art
[0002] With the development of UHV technology and miniaturization of electrical equipment, higher requirements are placed on the insulation performance of epoxy insulation materials. Therefore, further improvement of the insulation performance of epoxy resin materials is the key to improving the performance and reliability of power equipment. Epoxy resin has good insulation performance due to its wide bandgap, but this also leads to difficulties in the migration of space charges in epoxy insulation materials, which are easy to aggregate and cause distortion of the space electric field, limiting the further improvement of insulation performance.
[0003] Improving the insulation performance of epoxy insulating materials requires that they have a higher resistivity and improve the migration ability of space charges. In order to improve the insulation performance of epoxy resin materials, and at the same time make the space electric field uniform and prevent the distortion of the space electric field, domestic and foreign researchers have carried out a large number of experimental studies. Some researchers fluorinated the polymer surface by plasma etching, which enhanced the migration ability of charges on the surface and alleviated the accumulation of charges. The vacuum flashover voltage of the resin sample increased by 30%. Some researchers increased the charge migration rate and alleviated the distortion of the space electric field by plating a fluorinated layer on the surface of epoxy polymers. However, the optimization of insulation performance by surface treatment methods is limited to the surface of the material, and cannot improve the insulation performance of epoxy resin materials as a whole.
[0004] Some researchers have improved the surface flashover voltage of epoxy insulating materials by chain extension modification of epoxy resin molecules, but the surface resistivity and volume resistivity of the material decreased by 8.74% and 6.14%, respectively.
[0005] Chinese patent document CN 114015019 A A method for improving the surface flashover voltage of epoxy resin insulating materials, specifically including the following steps: S1 Preparation of fluorine-containing molecular fragments: Add trifluoride boron ether to water-free perfluorobutanol, add sodium hydroxide several times, and drop epichlorohydrin to carry out etherification reaction; add solvent benzene for extraction; filter the liquid and heat and distill to obtain perfluorobutanol glycidyl ether 7F-BGE; S2 Preparation of epoxy resin composite material: Mix epoxy resin, curing agent and perfluorobutanol glycidyl ether 7F-BGE according to a ratio, stir to obtain a uniformly dispersed casting material; perform vacuum degassing; obtain a standard test sample after curing and demolding; S3 Surface flashover voltage test. This technical solution is to increase the surface flashover voltage by fluorination. However, the existing method often brings about a decrease in resistivity when increasing the charge migration rate, and an excessive decrease in resistivity will affect the insulation performance of epoxy insulating materials.
[0006] Therefore, how to maintain the high resistivity of epoxy insulating materials while increasing their space charge migration rate is an important research topic for improving the insulation performance of epoxy insulating materials. It is necessary to develop a preparation method for high-insulating epoxy insulating materials based on fluorinated diluent modification, which can simultaneously improve insulation performance and good space charge migration ability. Summary of the invention
[0007] The purpose of the present invention is to provide a method for preparing a high-insulation epoxy insulating material based on fluorinated diluent modification, which improves the insulation strength of epoxy resin and achieves good space charge migration ability.
[0008] In order to solve the above technical problems, the technical solution adopted by the present invention is that the preparation method of the high-insulation performance epoxy insulation material based on fluorinated diluent modification specifically comprises the following steps:
[0009] S1 Preparation of fluorine-substituted modified BGE: trifluorobutanol or perfluorobutanol is added to a reaction vessel and reacted with boron trifluoride ether and epichlorohydrin in a heated environment for etherification. After the reaction is completed, the modified trifluorobutanol glycidyl ether 3F-BGE or perfluorobutanol glycidyl ether 7F-BGE is obtained by extraction, water washing and purification, and characterized;
[0010] Preparation of S2 epoxy insulation material samples: Mix the epoxy resin, curing agent and fluorine-substituted modified diluent in proportion, stir them fully under heating and vacuum conditions to obtain a uniformly dispersed casting material.
[0011] By adopting the above technical scheme, a fluorinated diluent is obtained by replacing modified butyl glycidyl ether (BGE) with fluorine atoms, and molecular orbital hybridization is achieved by replacing modified butyl glycidyl ether (BGE) with fluorine atoms, thereby modifying the existing epoxy resin system through the fluorinated diluent, improving the insulation performance of the epoxy insulating material, and optimizing the space charge migration ability of the epoxy insulating material.
[0012] Preferably, the specific steps of step S1 are:
[0013] S11: fractionate and purify trifluorobutanol or perfluorobutanol, and seal and store for later use;
[0014] S12: adding trifluorobutanol or perfluorobutanol and boron trifluoride ether to a reaction container, controlling the system temperature to remain constant, adding epichlorohydrin dropwise, and adding sodium hydroxide in multiple portions to carry out an etherification reaction;
[0015] S13: After the reaction is completed, benzene solution is added to the mixed liquid for extraction to obtain an upper oily liquid, and finally deionized water is used for multiple washings, and the obtained liquid is distilled and purified to obtain modified trifluorobutanol glycidyl ether 3F-BGE or perfluorobutanol glycidyl ether 7F-BGE.
[0016] Preferably, the step S1 further comprises step S14: structurally characterizing the obtained modified trifluorobutanol glycidyl ether 3F-BGE or perfluorobutanol glycidyl ether 7F-BGE to verify whether the diluent obtained by the reaction is the target product. The structural characterization of the obtained modified trifluorobutanol glycidyl ether 3F-BGE or perfluorobutanol glycidyl ether 7F-BGE is performed to prove that the reaction proceeds as expected and the obtained diluent is the target product.
[0017] Preferably, in step S11, trifluorobutanol or perfluorobutanol is heated in an oil bath to 110° C., stirred at a speed of 100 rad / min, and the fraction is purified and sealed for storage.
[0018] Preferably, in step S12, 1 to 3 mol of trifluorobutanol or perfluorobutanol and 0.02 to 0.10 mol of boron trifluoride ether are added to the reaction container, and the system temperature is controlled to be 50 to 70° C., 1 to 3 mol of epichlorohydrin is added dropwise, and a total amount of 1 to 3 mol of sodium hydroxide is added in multiple times to carry out etherification reaction, and the reaction time is 5 to 10 hours.
[0019] Preferably, in step S13, 10 mol of benzene solution is added to the mixed liquid for extraction to obtain an upper oily liquid, and finally deionized water is used for multiple washings, and the obtained liquid is distilled and purified to obtain modified trifluorobutanol glycidyl ether 3F-BGE or perfluorobutanol glycidyl ether 7F-BGE.
[0020] Preferably, the formula of the epoxy resin, curing agent and fluorine-substituted modified diluent in step S2 is as follows: 100 parts of epoxy resin, 84-85 parts of curing agent, 13-26 parts of diluent and 0.2-0.6 parts of accelerator.
[0021] Preferably, in step S2, the stirring rate is 300 rad / min, the temperature is 80° C., the vacuum degree is ≤100 Pa, and the time is 20 min, so as to obtain a uniformly dispersed casting material.
[0022] Preferably, the step S2 further includes curing the casting material to obtain a test sample.
[0023] Preferably, the specific steps of curing the castable in step S2 are: pouring the castable into a preheated mold and placing it in a blast oven, with a pre-curing temperature of 100°C and a time of 4 hours; a post-curing temperature of 140°C and a time of 12 hours, and obtaining a standard test sample after demolding.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] (1) Molecular orbital hybridization was achieved by using fluorine-substituted modified butyl glycidyl ether (BGE) to prepare a fluorine-substituted modified BGE active diluent;
[0026] (2) Use fluorinated diluents to modify the existing epoxy resin system, improve the insulation performance of epoxy insulation materials, optimize the spatial charge migration ability of epoxy insulation materials, prepare modified epoxy resin samples for performance testing and comparison, and verify the optimization of insulation performance of epoxy insulation materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The schematic diagram of the preparation of trifluorobutanol glycidyl ether 3F-BGE diluent in the preparation method of the high-insulation performance epoxy insulation material modified by fluorinated diluent of the present invention;
[0028] Figure 2 The schematic diagram of the preparation of the perfluorobutyl glycidyl ether 7F-BGE diluent in the preparation method of the high-insulation performance epoxy insulation material modified by the fluorinated diluent of the present invention;
[0029] Figure 3 The FTIR spectrum of the modified diluent in the method for preparing the high-insulation performance epoxy insulation material based on the modification of the fluorinated diluent of the present invention;
[0030] Figure 4 It is a mass fraction diagram of each element in the three diluents in the comparative example and specific examples 1 to 2 of the preparation method of the high-insulation performance epoxy insulation material modified by the fluorinated diluent of the present invention;
[0031] Figure 5 The present invention is a curing flow chart of a test sample of epoxy resin in the preparation method of the epoxy insulation material with high insulation performance modified by fluorinated diluent;
[0032] Figure 6The spatial charge distribution characteristics of the epoxy resin polymer over time in the preparation method of the high-insulating epoxy insulating material modified by the fluorinated diluent of the present invention; (a) is a diagram of the spatial charge distribution inside the material under an external continuous electric field of the comparative example; (b) is a diagram of the spatial charge distribution inside the material under an external continuous electric field of the specific example 1; (c) is a diagram of the spatial charge distribution inside the material under an external continuous electric field of the specific example 2;
[0033] Figure 7 The Weibull distribution diagram of the breakdown voltage of the epoxy polymer in the preparation method of the high-insulation performance epoxy insulation material modified by the fluorinated diluent of the present invention;
[0034] Figure 8 The volume resistivity and surface resistivity of the epoxy polymer in the preparation method of the high-insulation epoxy insulating material modified by the fluorinated diluent of the present invention. DETAILED DESCRIPTION
[0035] The technical solution is further described below in conjunction with the accompanying drawings.
[0036] Embodiment: A method for preparing a high-insulation epoxy insulating material modified by a fluorinated diluent, comprising the following steps:
[0037] S1 Preparation of fluorine-substituted modified BGE: trifluorobutanol or perfluorobutanol is added to a reaction vessel and reacted with boron trifluoride ether and epichlorohydrin in a heated environment for etherification. After the reaction is completed, the modified trifluorobutanol glycidyl ether 3F-BGE or perfluorobutanol glycidyl ether 7F-BGE is obtained by extraction, water washing and purification, and characterized;
[0038] The specific steps of step S1 are:
[0039] S11: fractionate and purify trifluorobutanol or perfluorobutanol, and seal and store for later use;
[0040] In the step S11, trifluorobutanol or perfluorobutanol is heated to 110° C. in an oil bath, stirred at a speed of 100 rad / min, and the fraction is purified and sealed for storage;
[0041] S12: adding trifluorobutanol or perfluorobutanol and boron trifluoride ether to a reaction container, controlling the system temperature to remain constant, adding epichlorohydrin dropwise, and adding sodium hydroxide in multiple portions to carry out an etherification reaction;
[0042] In the step S12, 1-3 mol of trifluorobutanol or perfluorobutanol and 0.02-0.10 mol of boron trifluoride ether are added to the reaction container, and the system temperature is controlled to be 50-70° C., and then 1-3 mol of epichlorohydrin is added dropwise, and a total amount of 1-3 mol of sodium hydroxide is added in multiple times to carry out etherification reaction, and the reaction time is 5-10 hours;
[0043] S13: After the reaction is completed, a benzene solution is added to the mixed solution for extraction to obtain an upper oily liquid, and finally the liquid is washed with deionized water for multiple times, and the obtained liquid is distilled and purified to obtain modified trifluorobutanol glycidyl ether 3F-BGE or perfluorobutanol glycidyl ether 7F-BGE;
[0044] In the step S13, 10 mol of benzene solution is added to the mixed solution for extraction to obtain an upper oily liquid, and finally deionized water is used for multiple washing, and the obtained liquid is distilled and purified to obtain modified trifluorobutanol glycidyl ether 3F-BGE or perfluorobutanol glycidyl ether 7F-BGE;
[0045] S14: structurally characterizing the obtained modified trifluorobutanol glycidyl ether 3F-BGE or perfluorobutanol glycidyl ether 7F-BGE to verify whether the diluent obtained by the reaction is the target product; structurally characterizing the obtained modified trifluorobutanol glycidyl ether 3F-BGE or perfluorobutanol glycidyl ether 7F-BGE to prove that the reaction proceeds as expected and the obtained diluent is the target product;
[0046] The specific results of the structural characterization of the fluorine-substituted modified diluent are:
[0047] The infrared spectrum of the diluent was analyzed using a Nicolet 67 Fourier transform infrared spectrometer from Thermo Nicolet. The results are as follows: Figure 3 As shown; at a wave number of 910cm -1 The peak is the epoxy group; at a wave number of 1100cm -1 The peak is the CO bond; at a wave number of 1180 cm -1 The peak is the CF bond; at a wave number of 1257 cm -1 The peak is the ether bond; at the wave number of 2850-2950cm -1 The peak -CH3 functional group at the bottom; the formation of ether bonds and the disappearance of -CH3 in the molecular structures of 3F-BGE and 7F-BGE indicate that F-containing butanol has undergone condensation reaction with epichlorohydrin, and since there are more CF bonds in 7F-BGE, its corresponding peak intensity is stronger than that of 3F-BGE;
[0048] The mass fractions of C, O, and F in the diluent were tested by organic element analyzer and hydrogen bomb titration. The results are as follows: Figure 4 As shown; Figure 4 The black percentage indicates the actual measured value, and the red percentage indicates the theoretical value of the target compound; with the increase of F atoms in the modified diluent molecule, its mass fraction increases from 0% to 31.97% and 52.11% respectively, and the results of the relative masses of C and O elements are basically consistent with the theoretical values of the target molecule; combined with the analysis of infrared spectra and the test of element content, it is believed that the two modified diluents 3F-BGE and 7F-BGE were successfully synthesized;
[0049] Preparation of S2 epoxy insulation material samples: epoxy resin, curing agent and fluorine-substituted modified diluent are mixed in proportion, and fully stirred under heating and vacuum conditions to obtain a uniformly dispersed casting material;
[0050] The formula of the epoxy resin, curing agent and fluorine-substituted modified diluent in step S2 is as follows: 100 parts of epoxy resin, 84-85 parts of curing agent, 13-26 parts of diluent and 0.2-0.6 parts of accelerator;
[0051] In step S2, the stirring rate is 300 rad / min, the temperature is 80° C., the vacuum degree is ≤100 Pa, and the time is 20 min, thereby obtaining a uniformly dispersed casting material;
[0052] The step S2 also includes curing the castable to obtain a test sample; the specific steps of curing the castable in the step S2 are: pouring the castable into the preheated mold and placing it in a blast oven, the pre-curing temperature is 100°C, the time is 4h; the post-curing temperature is 140°C, the time is 12h, and the standard test sample is obtained after demolding. Figure 5 shown.
[0053] Comparative Example: An epoxy resin test sample was prepared using unmodified diluent BGE, and the preparation method specifically includes the following steps:
[0054] Epoxy resin, curing agent and fluorine-substituted modified diluent were weighed according to the ratio, which were 100g epoxy resin, 84.66g curing agent, 13.01g diluent BGE and 0.5g accelerator respectively; epoxy resin, curing agent, diluent and accelerator were mixed, stirred at a rate of 300rad / min, temperature of 80℃, vacuum degree ≤100Pa, and time of 20min to obtain a uniformly dispersed casting material; the casting material was then poured into the preheated mold and placed in a blast oven, with a pre-curing temperature of 100℃ and a time of 4h; the post-curing temperature was 140℃ and a time of 12h, and a standard test specimen was obtained after demolding.
[0055] Specific Example 1: Using trifluorobutanol glycidyl ether 3F-BGE to prepare epoxy resin test samples, the preparation method specifically includes the following steps:
[0056] S1: Preparation of fluorine-substituted modified diluent; Figure 1 As shown;
[0057] S11: Heat trifluorobutanol or perfluorobutanol in an oil bath to 110°C, stir at a speed of 100 rad / min, purify the fraction, seal and store for later use; add 1 mol of trifluorobutanol or perfluorobutanol and 0.02 mol of boron trifluoride ether to a four-necked flask, control the system temperature to remain constant at 60°C, dropwise add 1 mol of epichlorohydrin, and add 50 g of sodium hydroxide several times, and etherify for 6 hours to obtain a mixed solution;
[0058] S12: After the reaction is completed, 10 mol of benzene solution is added to the mixed solution for extraction to obtain an upper oily liquid, and finally washed with deionized water for multiple times, and the obtained liquid is distilled and purified to obtain a modified diluent (3F-BGE or 7F-BGE);
[0059] S2: Preparation of epoxy insulation material samples;
[0060] Epoxy resin, curing agent and fluorine-substituted modified diluent were weighed according to the ratio, which were 100g epoxy resin, 84.66g curing agent, 18.41g diluent 3F-BGE and 0.5g accelerator respectively; epoxy resin, curing agent, diluent and accelerator were mixed, stirred at a rate of 300rad / min, temperature of 80℃, vacuum degree ≤100Pa, and time of 20min to obtain a uniformly dispersed casting material; the casting material was then poured into the preheated mold and placed in a blast oven, with a pre-curing temperature of 100℃ and a time of 4h; the post-curing temperature of 140℃ and a time of 12h, and a standard test specimen was obtained after demolding.
[0061] Specific Example 1: Perfluorobutyl glycidyl ether 3F-BGE is used to prepare epoxy resin test samples, and the preparation method specifically includes the following steps:
[0062] S1: Preparation of fluorine-substituted modified diluent; Figure 2 As shown;
[0063] S11: Heat the perfluorobutanol oil bath to 110°C, stir at 100 rad / min, purify the fraction, seal and store for later use; add 1 mol perfluorobutanol and 0.02 mol boron trifluoride ether to a four-necked flask, control the system temperature to remain constant at 60°C, dropwise add 1 mol epichlorohydrin, and add 50 g sodium hydroxide several times, and etherify for 6 hours to obtain a mixed solution;
[0064] S12: After the reaction is completed, 10 mol of benzene solution is added to the mixed solution for extraction to obtain an upper oily liquid, and finally washed with deionized water for multiple times, and the obtained liquid is distilled and purified to obtain a modified diluent (7F-BGE);
[0065] S2: Preparation of epoxy insulation material samples;
[0066] Epoxy resin, curing agent and fluorine-substituted modified diluent were weighed according to the ratio, which were 100g epoxy resin, 84.66g curing agent, 25.60g diluent 7F-BGE and 0.5g accelerator respectively; epoxy resin, curing agent, diluent and accelerator were mixed, stirred at a rate of 300rad / min, temperature of 80℃, vacuum degree ≤100Pa, and time of 20min to obtain a uniformly dispersed casting material; the casting material was then poured into the preheated mold and placed in a blast oven, with a pre-curing temperature of 100℃ and a time of 4h; the post-curing temperature of 140℃ and a time of 12h, and a standard test specimen was obtained after demolding.
[0067] The raw material proportions of the comparative example, specific example 1 and specific example 2 are shown in Table 1.
[0068] Table 1 Ratio of raw materials for preparing epoxy insulation materials
[0069] Example Epoxy resin(g) Curing agent (g) Diluent(g) Accelerator(g) Comparative Example 100 84.66 BGE 13.01 0.5 Specific embodiment 1 100 84.66 3F-BGE 18.41 0.5 Specific embodiment 2 100 84.66 7F-BGE 25.60 0.5
[0070] The comparative example, specific example 1 and specific example 2 were subjected to performance tests.
[0071] (1) The space charge migration ability of three epoxy polymers, namely, the comparative example (BGE / EP), the specific example 1 (3F-BGE / EP) and the specific example 2 (7F-BGE / EP), under a constant electric field was tested by using an electroacoustic pulse method (PEA). During the test, a 5 kV DC voltage was applied and the environment was placed at 25°C and 50% RH.
[0072] Figure 6 (a) Figure 6 (b) and Figure 6(c) in the figure are the spatial charge distribution diagrams of three epoxy polymers, namely the comparative example (BGE / EP), specific example 1 (3F-BGE / EP) and specific example 2 (7F-BGE / EP), under an external continuous electric field, wherein the electron density is greater at positions where the color is more red. As the electric field action time increases, a large number of electrons gather near the electrode inside the comparative example (BGE / EP), which will cause serious distortion of the electric field there. The electron density in specific example 1 (3F-BGE / EP) decreases slightly as the electric field action time increases, but charge accumulation still occurs in some areas. The electron density in specific example 2 (7F-BGE / EP) decreases significantly, and there is no area with significant electron accumulation. The test results show that compared with the comparative example (BGE / EP), the internal electron migration rate in specific example 1 (3F-BGE / EP) and specific example 2 (7F-BGE / EP) is significantly accelerated, thereby avoiding the large-scale accumulation of space charges. Modification of epoxy resin using the prepared fluorinated diluents 3F-BGE and 7F-BGE can improve the electron migration ability of epoxy insulating materials.
[0073] (2) The present invention tests the breakdown voltage and resistivity of the modified epoxy polymer. The results are as follows: Figure 7 , Figure 8 As shown, Figure 7 The Weibull distribution fitting curves of the breakdown voltages of three epoxy polymers, namely the comparative example (BGE / EP), the specific example 1 (3F-BGE / EP) and the specific example 2 (7F-BGE / EP), show that the breakdown strengths of the specific example 1 (3F-BGE / EP) and the specific example 2 (7F-BGE / EP) are increased by 7.74% and 11.34% compared to the unmodified comparative example (BGE / EP). At the same time, Figure 8 The volume resistivity and surface resistivity remain almost unchanged. The experimental results show that the epoxy insulation material modified by fluorinated diluent has higher insulation performance and good space charge migration ability.
[0074] The specific embodiments described above further illustrate the purpose, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention, such as changes in certain materials or reaction conditions, should be included in the scope of protection of the present invention.
Claims
1. A method for preparing a high-insulation epoxy insulating material modified by a fluorinated diluent, characterized in that: The specific steps include: S1 Preparation of fluorine-substituted modified BGE: trifluorobutanol or perfluorobutanol is added to a reaction vessel and subjected to etherification reaction with boron trifluoride ether and epichlorohydrin in a heated environment. After the reaction is completed, the modified trifluorobutanol glycidyl ether 3F-BGE or perfluorobutanol glycidyl ether 7F-BGE is obtained by extraction, washing and purification; Preparation of S2 epoxy insulation material samples: Mix the epoxy resin, curing agent and fluorine-substituted modified diluent in proportion, stir them fully under heating and vacuum conditions to obtain a uniformly dispersed casting material.
2. The method for preparing a high-insulation epoxy insulating material modified by a fluorinated diluent according to claim 1, characterized in that: The specific steps of step S1 are: S11: fractionate and purify trifluorobutanol or perfluorobutanol, and seal and store for later use; S12: adding trifluorobutanol or perfluorobutanol and boron trifluoride ether to a reaction container, controlling the system temperature to remain constant, adding epichlorohydrin dropwise, and adding sodium hydroxide in multiple portions to carry out an etherification reaction; S13: After the reaction is completed, benzene solution is added to the mixed liquid for extraction to obtain an upper oily liquid, and finally deionized water is used for multiple washings, and the obtained liquid is distilled and purified to obtain modified trifluorobutanol glycidyl ether 3F-BGE or perfluorobutanol glycidyl ether 7F-BGE.
3. The method for preparing a high-insulation epoxy insulating material modified by a fluorinated diluent according to claim 2, characterized in that: The step S1 also includes step S14: structurally characterizing the obtained modified trifluorobutanol glycidyl ether 3F-BGE or perfluorobutanol glycidyl ether 7F-BGE to verify whether the diluent obtained by the reaction is the target product.
4. The method for preparing a high-insulation epoxy insulating material based on fluorinated diluent modification according to claim 2, characterized in that: In the step S11, trifluorobutanol or perfluorobutanol is heated in an oil bath to 110° C., stirred at a speed of 100 rad / min, and the fraction is purified and sealed for storage.
5. The method for preparing a high-insulation epoxy insulating material modified by a fluorinated diluent according to claim 4, characterized in that: In the step S12, 1-3 mol of trifluorobutanol or perfluorobutanol and 0.02-0.10 mol of boron trifluoride ether are added to the reaction container, and the system temperature is controlled to be constant at 50-70° C., and then 1-3 mol of epichlorohydrin is added dropwise, and a total amount of 1-3 mol of sodium hydroxide is added in multiple times to carry out etherification reaction, and the reaction time is 5-10 hours.
6. The method for preparing a high-insulation epoxy insulating material modified by a fluorinated diluent according to claim 5, characterized in that: In the step S13, 10 mol of benzene solution is added to the mixed liquid for extraction to obtain an upper oily liquid, and finally deionized water is used for multiple washing, and the obtained liquid is distilled and purified to obtain the modified trifluorobutanol glycidyl ether 3F-BGE or perfluorobutanol glycidyl ether 7F-BGE.
7. The method for preparing a high-insulation epoxy insulating material based on fluorinated diluent modification according to claim 2, characterized in that: The formula of the epoxy resin, curing agent and fluorine-substituted modified diluent in step S2 is as follows: 100 parts of epoxy resin, 84-85 parts of curing agent, 13-26 parts of diluent and 0.2-0.6 parts of accelerator.
8. The method for preparing a high-insulation epoxy insulating material modified by a fluorinated diluent according to claim 7, characterized in that: In step S2, the stirring rate is 300 rad / min, the temperature is 80° C., the vacuum degree is ≤100 Pa, and the time is 20 min, thereby obtaining a uniformly dispersed casting material.
9. The method for preparing a high-insulation epoxy insulating material modified by a fluorinated diluent according to claim 7, characterized in that: The step S2 also includes solidifying the casting material to obtain a test sample.
10. The method for preparing a high-insulation epoxy insulating material based on fluorinated diluent modification according to claim 9, characterized in that: The specific steps of curing the castable in step S2 are: pouring the castable into the preheated mold and placing it in a blast oven, with a pre-curing temperature of 100° C. and a time of 4 hours; a post-curing temperature of 140° C. and a time of 12 hours, and obtaining a standard test sample after demoulding.
Citation Information
Patent Citations
Fluorine-containing epoxide resin reactive diluent and preparation thereof
CN101353331A
Method for increasing surface flashover voltage of epoxy resin insulating material
CN114015019A
Reactive diluents for epoxy resins
GB1044142A
Epoxy resin system having phase separation structure, preparation method therefor and application thereof
US20230024059A1
Radiation-resistant fluorine-silicon containing epoxy-resin coating and preparation method thereof
WO2017166913A1
Cited By
Epoxy material for large-size direct-current insulating part and preparation method of epoxy material
CN121022032A
Epoxy resin insulating material with high toughness and high breakdown field strength as well as preparation method and application of epoxy resin insulating material
CN121226684A