Method for efficiently preparing single-walled carbon nanotubes
Single-wall carbon nanotubes were prepared by loading catalytically active particles on molecular sieve and using chemical vapor deposition method. Combined with ultrasonic treatment and vacuum separation, the problems of low yield and low G/D ratio of single-wall carbon nanotube preparation were solved, and the problem of low yield and low G/D ratio was achieved. It can provide high efficiency, low cost, high yield and high G/D ratio preparation to meet the conductivity requirements of lithium-ion batteries.
Patent Information
- Application Number
- CN202310616683.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-29
- Publication Date
- 2024-11-29
AI Technical Summary
The existing single-wall carbon nanotube preparation process has the problems of low carbon tube yield and low G/D ratio, which is difficult to meet the conductivity needs of lithium-ion batteries.
Catalytic active particles are supported on molecular sieve to prepare catalysts, single-walled carbon nanotubes are prepared on the catalyst surface by chemical vapor deposition, and ultrasonic treatment and vacuum separation are carried out in acidic solution to improve yield and G/D ratio.
It realizes efficient preparation of single-wall carbon nanotubes with high yield and high G/D ratio, improves the carbon tube magnification and conductivity, reduces the preparation cost, and the molecular sieve can be recycled.
Smart Images

Figure HDA0004254072730000011 
Figure HDA0004254072730000012 
Figure HDA0004254072730000021
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of carbon nanotubes, and more specifically, to a method for efficiently preparing single-walled carbon nanotubes. Background Art
[0002] As a nanomaterial, carbon nanotubes have excellent electrical conductivity, thermal conductivity and mechanical properties, and are used in many fields such as chemical industry, aerospace, and medical treatment. In recent years, due to the obvious performance advantages of carbon nanotubes used as conductive agents for lithium batteries, the market demand for carbon nanotubes has increased year by year. With the increase in the energy density of lithium-ion batteries, more and more silicon-based negative electrodes are used in lithium-ion batteries. However, compared with graphite negative electrode materials, silicon-based negative electrode materials have poor electrical conductivity. In order to achieve the same electrical conductivity, single-walled carbon nanotubes with better conductivity are needed as conductive additives. Chemical vapor deposition is a relatively easy method for large-scale preparation, but the current single-walled tube preparation process has the problems of low carbon tube yield (multiplier <1) and low G / D ratio (G / D <10). Summary of the invention
[0003] In order to improve the yield and G / D in the preparation process of single-walled carbon nanotubes, the present application provides a method for efficiently preparing single-walled carbon nanotubes.
[0004] The present application provides a method for efficiently preparing single-walled carbon nanotubes, which adopts the following technical scheme: catalytically active particles are loaded on a molecular sieve to obtain a catalyst, and then single-walled carbon nanotubes are obtained on the surface of the catalyst by chemical vapor deposition, and then ultrasonically immersed in an acidic solution, filtered and dried, and finally the catalyst and the carbon nanotubes are separated by a vacuum system.
[0005] The catalyst precursor hydroxide is prepared by hydrothermal method, then calcined in air, and the catalytic active particles are loaded on the molecular sieve to obtain the catalyst. The Al atoms on the molecular sieve act as acidic sites and have an adsorption effect on the catalytic active center. During the reaction, the catalytic activity of the catalytic active center can be maintained, thereby improving the rate and G / D ratio.
[0006] A single-walled carbon nanotube solid product is obtained on the catalyst surface by chemical vapor deposition, and the solid product includes a molecular sieve catalyst and the generated single-walled carbon nanotubes. The solid product is placed in an acidic solution for ultrasonic treatment to fully dissolve the catalyst on the surface of the molecular sieve, so that the single-walled carbon nanotubes are peeled off from the surface of the molecular sieve. Then, suction filtration and drying are performed to obtain a mixture of the molecular sieve and the single-walled carbon nanotubes. The single-walled carbon nanotubes can be easily collected using a vacuum system, and the remaining molecular sieve can be recycled. This method can be used to efficiently and cheaply prepare single-walled carbon nanotubes with high yield and G / D ratio in large quantities.
[0007] Preferably, the method for loading the catalytically active particles on the molecular sieve to obtain the catalyst is to place the layered molecular sieve in water or an organic solvent, add a metal salt containing the metal element in the catalytically active particles, the mass ratio of the metal salt to the molecular sieve is preferably 0.005-0.2:1, and the pH of the solution is adjusted to be alkaline. After the hydrothermal reaction is completed, the solid particles are filtered and calcined to obtain a catalyst for preparing single-walled carbon nanotubes. Among them, the metal salt containing the catalyst is preferably a sulfate or nitrate containing iron, cobalt, and nickel. After the metal salt is mixed with the molecular sieve, the pH value of the solution needs to be adjusted, preferably to 7-10. Under the above pH conditions, the metal salt is more easily and evenly deposited on the surface of the molecular sieve.
[0008] Under hydrothermal conditions, metal salts will undergo hydrolysis to generate hydroxides, and the Al on the molecular sieve, as an acidic site, will interact with metal ions and act as an anchor, making it easier for metal ions to deposit around Al and decompose into hydroxides.
[0009] Preferably, the catalytically active particles are one or more of Fe oxide, Co oxide and Ni oxide.
[0010] Preferably, the layered zeolite molecular sieve includes ZSM-5 or SAPO-34.
[0011] Preferably, after the reactor reaches the target temperature, the carbon source is introduced for 30-60 minutes.
[0012] Preferably, the layered zeolite molecular sieve comprises ZSM-5 or SAPO-34. The Si / Al ratio of the layered zeolite molecular sieve is greater than 90, preferably 100-170, and more preferably 100-150. In the subsequent treatment process of the reaction, if the Al content in the molecular sieve is too high, the structure of the molecular sieve itself will be destroyed.
[0013] Preferably, the hydrothermal reaction is carried out at a temperature of 150-300°C for a time of 0.5-24 hours. Preferably, the calcination reaction is carried out at a temperature of 300-700°C for a time of 1-2 hours.
[0014] Preferably, the chemical vapor deposition method for preparing single-walled carbon nanotubes uses a fixed bed to carry out the reaction to obtain the target product.
[0015] Preferably, the chemical vapor deposition method for preparing single-walled carbon nanotubes is to control the particle size of the catalyst by spray granulation so that the particle size D 50 Between 30-300 μm, the reaction can be carried out in a fluidized bed reactor.
[0016] Preferably, the reaction temperature of the chemical vapor deposition method for preparing single-walled carbon nanotubes is maintained between 850-1400° C. During the reaction, the total proportion of H2 introduced to the introduced gas is in the range of 2-15 vol%, the total proportion of the introduced carbon source is in the range of 0.5-15 vol%, and the remaining gas is inert protective gas such as N2 and Ar.
[0017] Preferably, in the initial stage of the chemical vapor deposition reaction for preparing single-walled carbon nanotubes, no carbon source is introduced, only H2 and N2 are introduced to reduce the active substances on the surface of the molecular sieve to obtain a catalyst with catalytic activity, and the duration is 5-30 minutes.
[0018] Preferably, the ultrasonic immersion time is 30 min-2 h; the pH value of the acidic solution does not exceed 1.5. Within this pH range, the metal impurities in the carbon nanotubes can be effectively removed. Too high a pH value will result in insufficient removal of the metal impurities. During the filtration process, an appropriate amount of water is added to make the pH of the carbon nanotube solution 6.8-7.6. By controlling the pH value within this range, the H + Remove.
[0019] In summary, this application has the following beneficial effects: 1. The present application designs a catalyst and uses chemical vapor deposition to achieve batch preparation of single-walled carbon nanotubes, thereby increasing the carbon tube yield (multiplier>10) and further increasing the G / D ratio of single-walled carbon nanotubes (G / D>20).
[0020] 2. The present invention can easily remove the metal catalyst in the single-walled tube through a simple acid washing process. At the same time, the carrier molecular sieve used in the process can be recycled, thereby effectively reducing the cost of preparing single-walled carbon nanotubes. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is the SEM image of the catalyst ground to less than 400 mesh; Figure 2 This is a TEM image of the catalyst ground to less than 400 mesh; Figure 3 This is a typical single-walled carbon nanotube characteristic diagram, with a G / D ratio of 85; Figure 4 This is a TEM image of a single-walled carbon nanotube, with a diameter of about 2.1 nm; Figure 5 It is the relationship diagram of G / D changing with Si / Al ratio; Figure 6 It is the relationship diagram of the ratio changing with Si / Al ratio; Figure 7 The relationship between the rate and Si / Al and the number of reactions. DETAILED DESCRIPTION
[0022] Example 1 10g ZSM-5 molecular sieve (Si / Al=150) was dispersed in 200ml pure water, 10ml 0.1mol / L cobalt nitrate solution was added dropwise to the suspension, pH was adjusted to 7.5, stirred for 30min, the solution was placed in a 500ml hydrothermal kettle, reacted at 150°C for 2h, cooled to room temperature, filtered to obtain a catalyst precursor (cobalt hydroxide), and then calcined in air at 300°C for 1.5h to obtain a catalyst (molecular sieve loaded with cobalt oxide), and the obtained catalyst was ground to 30-80μm in a mortar. The SEM and TEM photos of the prepared catalyst are shown in Figure 2. Figure 1 , Figure 2 shown.
[0023] Take 0.1g of catalyst, put it into a quartz boat and place it in the high temperature zone of the tube furnace. Connect the gas line, introduce nitrogen at a flow rate of 2L / min. Start heating after 10min and raise the temperature to 1000℃ at a rate of 30℃ / min. After the temperature reaches the reaction target temperature of 1000℃, introduce 0.2L / min of H2 and maintain it for 5min; then introduce 0.2L / min of CH4 and keep warm for 30min; then continue to pass nitrogen at 1L / min until it drops to room temperature.
[0024] After the sample is cooled, the solid particles obtained are weighed to obtain 2.6g of a mixture of carbon nanotubes and catalysts, and the calculated multiplier is 25 times. The obtained solid powder is immersed in 100ml of 10mol / L H2SO4 solution, reacted (ultrasonic immersion) for 2h, and then filtered and dried. Water is added during the filtration process to make the pH value of the carbon tube solution 6.8, and molecular sieves and single-walled carbon nanotubes are obtained. Since single-walled carbon nanotubes are relatively light, they can be easily extracted by a vacuum device, thereby achieving separation from the molecular sieve. Finally, 2g of single-walled carbon nanotubes are obtained. Figure 3 As shown, it is a typical single-walled carbon nanotube feature with a G / D ratio of 85. Figure 4 To prepare TEM photos of single-walled carbon nanotubes, it can be seen from the TEM photos that their diameter is approximately 2.1nm.
[0025] Example 2 10g ZSM-5 molecular sieve (Si / Al=80) was dispersed in 200ml pure water, 10ml 0.1mol / L ferric nitrate solution was added dropwise to the suspension, the pH was adjusted to 7.5, and after stirring for 30min, the solution was placed in a 500ml hydrothermal autoclave, reacted at 300°C for 2h, and after cooling to room temperature, filtered to obtain a catalyst precursor (ferric hydroxide), and then calcined in air at 600°C for 1h to obtain a catalyst (molecular sieve loaded with iron oxide), and the obtained catalyst was ground to 30-80μm in a mortar.
[0026] Take 0.2g of catalyst, put it into a quartz boat and place it in the high temperature zone of the tube furnace. Connect the gas line, introduce nitrogen at a flow rate of 5L / min. Start heating after 10min and raise the temperature to 1400℃ at a rate of 20℃ / min. After the temperature reaches the reaction target temperature of 1400℃, introduce 0.3L / min of H2 and maintain for 30min; then introduce 0.6L / min of CH4 and keep warm for 30min; then continue to pass nitrogen at 1L / min until it drops to room temperature.
[0027] After the sample is cooled, the solid particles obtained are weighed to obtain a mixture of 8.2g carbon nanotubes and catalysts, and the calculation ratio is 40 times. The obtained solid powder is immersed in 100ml 1.5mol / L H2SO4 solution, and the reaction (ultrasonic immersion) is filtered and dried after 2h. Water is added during the filtration process to make the pH value of the carbon tube solution 7.6, and molecular sieves and single-walled carbon nanotubes are obtained. Since single-walled carbon nanotubes are relatively light, single-walled carbon nanotubes can be easily extracted by a vacuum device, thereby separating them from molecular sieves. Finally, 6g single-walled carbon nanotubes are obtained. The carbon nanotube G / D ratio is 8, and its diameter is about 2.5nm.
[0028] Example 3 10g ZSM-5 molecular sieve (Si / Al=170) was dispersed in 200ml pure water, 10ml 0.1mol / L nickel nitrate solution was added dropwise to the above suspension, the pH was adjusted to 7.5, and after stirring for 30min, the above solution was placed in a 500ml hydrothermal autoclave, reacted at 220°C for 1.5h, and after cooling to room temperature, filtered to obtain a catalyst precursor (nickel hydroxide), and then calcined at 700°C in air for 2h to obtain a catalyst (molecular sieve loaded with nickel oxide), and the obtained catalyst was ground to 80-300μm in a mortar.
[0029] Take 0.5g of catalyst, put it into a quartz boat and place it in the high temperature zone of the tube furnace. Connect the gas line, introduce nitrogen at a flow rate of 10L / min. Start heating after 10min and raise the temperature to 850℃ at a rate of 20℃ / min. After the temperature reaches the reaction target temperature of 850℃, introduce 0.25L / min of H2 and maintain it for 25min; then introduce 0.25L / min of CH4 and keep it warm for 60min; then continue to pass nitrogen at 2L / min until it drops to room temperature.
[0030] After the sample is cooled, the solid particles obtained are weighed to obtain a mixture of 6.5g carbon nanotubes and catalysts, and the calculation ratio is 12 times. The obtained solid powder is immersed in 100ml 1mol / L H2SO4 solution, and the reaction (ultrasonic immersion) is filtered and dried after 2h. Water is added during the filtration process to make the pH value of the carbon tube solution 7.0, and molecular sieves and single-walled carbon nanotubes are obtained. The single-walled carbon nanotubes are easily removed by a vacuum device, thereby separating them from the molecular sieve. Finally, 4g single-walled carbon nanotubes are obtained. The carbon nanotube G / D ratio is 90, and its diameter is about 1.8nm.
[0031] The difference between Examples 4 and 5 and Example 1 is that Si / Al is different, and other parameters remain unchanged. The results are shown in Table 1.
[0032] Comparative Example Method for preparing single-walled carbon nanotubes using conventional technology The catalyst preparation process and reaction conditions are the same as those in Example 1, except that the carrier is changed to magnesium oxide, and the magnesium-containing solution and single-walled carbon nanotubes are obtained after acid washing. The reaction ratio is 0.8, and 0.05g of single-walled carbon nanotubes are finally obtained, with a G / D ratio of 0.8 and a diameter of about 3nm.
[0033] Table 1 Example Si / Al G / D First magnification Second magnification The third multiplier 1 150 85 25 22 20 2 80 8 40 8 2 3 170 90 12 6 3 4 100 22 42 35 28 5 130 64 31 28 26 Comparative Example - 0.8 0.8 - - like Figure 5 As shown, the Si / Al of the molecular sieve was adjusted to 80, 100, 130, 150 and 170 respectively, and the other parameters remained unchanged. The G / D values of the prepared carbon nanotubes were 8, 22, 64, 85 and 90 respectively.
[0034] like Figure 5 As shown, with the increase of Si / Al ratio, the number of Al atoms serving as acidic sites decreases, resulting in a decrease in the positions for adsorbing oxide active sites, making the oxide active sites evenly dispersed, thereby effectively improving the G / D ratio.
[0035] like Figure 6 As shown in the figure, with the increase of Si / Al ratio, the acidic sites become fewer and fewer, and the corresponding number of loaded oxide active sites will also decrease, which will affect the rate performance.
[0036] When Si / Al is 80, due to the high aluminum content in the molecular sieve, in the subsequent stripping process of single-walled carbon nanotubes and molecular sieves, the aluminum in the molecular sieve, especially the aluminum located on the surface of the molecular sieve, will be easily lost after acid treatment, which will lead to a rapid decrease in the rate performance of the molecular sieve for secondary, tertiary or more growth of single-walled carbon nanotubes.
[0037] like Figure 7 As shown, with the increase of Si / Al ratio, the stability of molecular sieve in acidic solution becomes higher and higher, making the active site of molecular sieve more stable. It can be seen that when Si / Al is between 100-150, the catalyst made after two cycles of molecular sieve can still obtain a rate performance greater than 20.
[0038] It can be seen from the comparative examples that the catalyst prepared by the method of this patent significantly improves the carbon tube rate.
[0039] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A method for efficiently preparing single-walled carbon nanotubes, characterized in that: The catalyst is obtained by loading catalytically active particles on a molecular sieve, and then single-walled carbon nanotubes are obtained on the catalyst surface by chemical vapor deposition. The catalyst is then ultrasonically immersed in an acidic solution, filtered, dried, and finally separated from the carbon nanotubes by a vacuum system.
2. The method for efficiently preparing single-walled carbon nanotubes according to claim 1, characterized in that: The method for loading catalytically active particles on molecular sieves to obtain a catalyst is to place a layered zeolite molecular sieve in water or an organic solvent, add a metal salt containing the metal element in the catalytically active particles, adjust the pH of the solution to be alkaline, and after the hydrothermal reaction is completed, filter and calcine to obtain the catalyst.
3. The method for efficiently preparing single-walled carbon nanotubes according to claim 1 or 2, characterized in that: The catalytically active particles are one or more of Fe oxide, Co oxide and Ni oxide.
4. The method for efficiently preparing single-walled carbon nanotubes according to claim 1 or 2, characterized in that: The layered zeolite molecular sieve includes ZSM-5 or SAPO-34.
5. The method for efficiently preparing single-walled carbon nanotubes according to claim 2, characterized in that: The Si / Al ratio of the layered zeolite molecular sieve is 100-170.
6. The method for efficiently preparing single-walled carbon nanotubes according to claim 2, characterized in that: The hydrothermal reaction conditions are a temperature of 150 o C-300 o C, the calcination reaction condition is a temperature of 150-700°C.
7. The method for efficiently preparing single-walled carbon nanotubes according to claim 1, characterized in that: The target reaction temperature of the chemical vapor deposition method for preparing single-walled carbon nanotubes is maintained between 850-1400°C.
8. The method for efficiently preparing single-walled carbon nanotubes according to claim 2, characterized in that: The mass ratio of the metal salt to the molecular sieve is 0.005-0.2:
1.
9. The method for efficiently preparing single-walled carbon nanotubes according to claim 1, characterized in that: The pH value of the acidic solution does not exceed 1.
5.
10. The method for efficiently preparing single-walled carbon nanotubes according to claim 1, characterized in that: The particle size D50 of the catalyst is 30-300 μm.
Citation Information
Patent Citations
Method for preparing single walled carbon nanotubes
CN101103150A
Method of forming single-walled carbon nanotubes
CN102548896A
Preparation method of single-walled carbon nanotube
CN107601458A
Method for catalytic preparation of carbon nanotubes with empty-shell type small grain ZSM-5 molecular sieve loaded metal
CN110228803A
Composition containing single-walled carbon nanotube
JP2007070224A
Cited By
Process for preparing single-walled carbon nanotubes and graphene by stripping multi-walled carbon nanotubes