Binder for ceramics and electronic ceramic component

By using polyvinyl acetal resin as the binder for ceramic capacitors and controlling its conductivity during the manufacturing process, the problem of high ash and metal content in ceramic capacitors is solved, and the electrical performance is improved.

CN119039015APending Publication Date: 2024-11-29ZHEJIANG DECENT PLASTIC

Patent Information

Application Number
CN202411529012.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-30
Publication Date
2024-11-29

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to the field of binders, in particular to a binder for ceramics and an electronic ceramic component. The binder for ceramics is used in the ceramic manufacturing process, the binder comprises thermoplastic resin, and the thermoplastic resin at least comprises polyvinyl acetal resin; the binder is prepared into a deionized water solution or dispersion solution with the mass fraction of 10%, and the conductivity of the binder is smaller than or equal to 100 [mu] S / cm at the temperature of 25 DEG C. According to the ceramic binder and the electronic ceramic component provided by the invention, the conductivity of the polyvinyl acetal resin in the deionized water is controlled, so that the polyvinyl acetal as the binder is low in ash content and low in metal component content in a preparation process of a ceramic capacitor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of adhesives, and in particular to an adhesive for ceramics and an electronic ceramic component. Background Art

[0002] With the rapid development of the electronics industry, the types and quantities of electronic components are increasing. Electronic ceramics are gradually being used in electronic components due to their electrical and magnetic properties. Among them, ceramic capacitors are widely used in DC isolation, coupling, bypass, filtering, tuning circuits, energy conversion and control circuits due to their advantages such as large capacity range, low equivalent series resistance, high rated voltage and good high-frequency characteristics, becoming important electronic components. At present, circuits in the fields of electronics, communications, aerospace, etc. are gradually becoming miniaturized and integrated. Multilayer ceramic capacitors are capacitors with inner electrode layers and ceramic dielectric layers interlaced and superimposed, and end electrodes (external electrodes) are led out to form a parallel structure.

[0003] The preparation process of multilayer ceramic capacitors generally includes: batching, casting, printing, stacking, lamination, cutting, debinding, sintering, grinding, capping, sintering and electroplating. Among them, the batching process is to ball-mill or sand-mill the ceramic powder, binder, solvent and various additives in a certain proportion for a certain period of time to form a uniform and stable ceramic slurry; debinding is to heat-treat the ceramic green body after cutting to remove organic matter such as binders. During the debinding process, if there is ash formed by residual carbon, it will cause defects such as stratification and cracking of the ceramic green body during the sintering stage; at the same time, if the debinding stage is not thorough, the residual ash and metal components will affect the electrical properties of the ceramic capacitor.

[0004] In the prior art, patent CN 118139925 A discloses a polyvinyl acetal resin composition, an inorganic particle dispersion slurry composition, and a laminated ceramic capacitor. The polyvinyl acetal resin composition has a water content of 5.0% by weight or less. The polyvinyl acetal composition contains a polyvinyl acetal resin and a compound A. Compound A contains carbon, hydrogen, and oxygen atoms, and the ratio of the number of oxygen atoms to the total number of atoms is greater than 0.18. Patent CN 118055974 A discloses a polyvinyl acetal resin composition, an inorganic particle dispersion carrier composition, an inorganic particle dispersion slurry composition, and a laminated ceramic capacitor. In order to reduce the content of residue or residual carbon, the content of polyvinyl acetal resin in the inorganic particle dispersion slurry composition is greater than 2% by weight and less than 30% by weight; the inorganic particle dispersion slurry composition contains a plasticizer, and the boiling point of the plasticizer is greater than 240°C and less than 390°C.

[0005] In order to solve the above problems, at present, there is an urgent need to invent a ceramic binder and an electronic ceramic component to solve the problem of high ash and metal content in the electronic ceramic component during the manufacturing process of the electronic ceramic. Summary of the invention

[0006] When polyvinyl acetal resin is used as a binder for electronic components, the binder removal process often results in incomplete binder removal and excessively high residual ash, which affects the electrical properties of the electronic components, especially the manufactured ceramic capacitors. Therefore, the present invention aims to solve the problem of high ash content in ceramic binders.

[0007] A first aspect of the present invention provides a ceramic binder, which is used in a ceramic manufacturing process. The binder includes a thermoplastic resin, and the thermoplastic resin includes at least a polyvinyl acetal resin. The binder is formulated into a deionized water solution or a dispersed solution with a mass fraction of 10%, and its electrical conductivity is ≤100μS / cm at 25°C.

[0008] It should be noted that the binder is formulated into a deionized water solution or dispersed solution with a mass fraction of 10%, which means that 10 parts by weight of the binder is added to 90 parts by weight of deionized water and stirred thoroughly to obtain a product. If the binder is water-soluble, the product is a clear and transparent aqueous solution. If the binder is insoluble in water or partially soluble in water, the product is a dispersed liquid. During the stirring process, in order to achieve the effect of sufficient dissolution or dispersion, methods such as increasing the temperature, high-speed stirring, and ultrasonic vibration can be used, and then the conductivity is measured at 25°C to be ≤100μS / cm.

[0009] The inventors have found that by meeting the above conductivity requirements, the ash content can be effectively reduced or the generation of ash can be avoided in the manufacture of ceramic capacitors; at the same time, it is also found that the binder meets the above conductivity requirements and can effectively reduce the content of metal components in the manufacture of ceramic capacitors (metal components are inevitable metal components introduced in the preparation or synthesis of binders or in the preparation of ceramic capacitors, etc. The inventors have found that in the prior art, some metal components are also present in the use of polyvinyl acetal resin as a binder for ceramic capacitors, and the metal components affect the electrical properties of ceramic capacitors).

[0010] The thermoplastic resin described above may include only polyvinyl acetal resin; or it may be a mixture of polyvinyl acetal resin and other thermoplastic resins. For example, other thermoplastic resins include one or more of ethylene-vinyl acetate copolymer resin, ethylene-acrylic acid copolymer resin, polyurethane resin, polyvinyl alcohol resin, polyester resin, and methacrylic acid copolymer resin; the ratio of polyvinyl acetal resin to other thermoplastic resins is not limited here, as long as the above-mentioned conductivity ≤100μS / cm is satisfied.

[0011] Preferably, the binder is formulated into a 10% by mass deionized water solution or dispersed solution, and its conductivity is ≤50 μS / cm at 25° C.

[0012] According to the ceramic binder as described above provided by the present invention, the binder is formulated into an ethanol solution with a mass fraction of 10% (i.e., a product obtained by adding 10 parts by weight of the binder to 90 parts by weight of ethanol and stirring sufficiently. During the stirring process, in order to achieve the effect of sufficient dissolution, methods such as increasing the temperature, high-speed stirring, and ultrasonic vibration can be adopted). At 25°C, the conductivity of its 10% ethanol solution is ≤50μS / cm; preferably, the conductivity of its 10% ethanol solution is ≤30μS / cm.

[0013] According to the ceramic binder as described above provided by the present invention, the binder is baked at 180°C for 1 hour, and its b value is ≤5; preferably, the binder is baked at 180°C for 1.5 hours, and its b value is ≤5; more preferably, the binder is baked at 180°C for 2 hours, and its b value is ≤5.

[0014] According to the ceramic binder provided by the present invention, the binder is prepared into an ethanol solution with a mass fraction of 10%, and the viscosity of the 10% ethanol solution is ≤500mPa·s at 25°C; Or / and, the binder is prepared into an ethanol solution with a mass fraction of 30%, and the viscosity of the 30% ethanol solution is ≤70000 mPa·s at 25°C.

[0015] Preferably, the binder is prepared into an ethanol solution with a mass fraction of 10%, and at 25°C, the solution adhesive viscosity is 20mPa·s≤≤200mPa·s.

[0016] Preferably, the binder is formulated into an ethanol solution with a mass fraction of 30%, and the viscosity of the 30% ethanol solution is ≤50000 mPa·s at 25°C; more preferably, the binder is formulated into an ethanol solution with a mass fraction of 30%, and the viscosity of the 30% ethanol solution is ≤30000 mPa·s at 25°C.

[0017] According to the ceramic binder as described above provided by the present invention, the glass transition temperature of the binder is ≥40°C; preferably, the glass transition temperature of the binder is ≥55°C; more preferably, the glass transition temperature of the binder is ≥60°C.

[0018] According to the ceramic binder as described above provided by the present invention, the maximum thermal decomposition temperature of the binder is ≤450°C; preferably, the maximum thermal decomposition temperature of the binder is ≤430°C; more preferably, the maximum thermal decomposition temperature of the binder is ≤420°C.

[0019] According to the ceramic binder provided by the present invention, the polyvinyl acetal resin is formed by condensation of polyvinyl alcohol and aldehyde compounds under acid catalysis conditions.

[0020] According to the ceramic binder provided by the present invention, an antioxidant is added to the polyvinyl acetal resin during the condensation process; preferably, the antioxidant includes one or a mixture of phenolic antioxidants and phosphate antioxidants.

[0021] According to the ceramic binder as described above provided by the present invention, the number of carbon atoms in the molecular formula of the aldehyde compound is 2-8 and the number of oxygen atoms is 1-3; or / and the mass content of hydroxyl groups in the polyvinyl acetal resin is 13%-26%.

[0022] A second aspect of the present invention provides an electronic ceramic component, which is prepared using the ceramic binder provided by the present invention as described above.

[0023] According to the electronic ceramic component as described above provided by the present invention, the electronic ceramic component includes a ceramic capacitor or a ceramic substrate.

[0024] Compared with the prior art, the present invention has the following technical effects: the ceramic binder and electronic ceramic components provided by the present invention control the conductivity of polyvinyl acetal resin in deionized water, so that polyvinyl acetal is used as a binder in the preparation process of ceramic capacitors with low ash content and low metal component content. DETAILED DESCRIPTION

[0025] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without carrying out creative work are within the scope of protection of the present invention.

[0026] In the description of the present invention, it should be understood that the component fractions of the deionized water solution or dispersed solution and the ethanol solution, etc., all represent mass fractions unless otherwise specified.

[0027] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0028] The more complete the debinding of ceramic capacitors during the manufacturing process, the lower the residual ash and metal components in the ceramic capacitors, and the better the electrical performance of the ceramic capacitors.

[0029] In the related art, the ash content is mostly reduced by adding other components to the binder or controlling the amount of the binder.

[0030] However, in the process of practicing the present invention, the inventors found that controlling the conductivity of the binder in deionized water is helpful to reduce the ash content and can also reduce the content of metal components at the same time.

[0031] The present invention provides a ceramic binder, which is used in a ceramic manufacturing process. The binder includes a thermoplastic resin and an antioxidant, and the thermoplastic resin includes at least a polyvinyl acetal resin. The binder is formulated into a deionized water solution or a dispersion solution with a mass fraction of 10%, and its conductivity is ≤100μS / cm at 25°C. The formulation of the 10% deionized water solution or dispersion solution recorded here means that if the binder is water-soluble, it is formulated into an aqueous solution, and if the binder is insoluble in water or partially soluble in water, it is formulated into a dispersion solution; illustratively, the thermoplastic resin only includes the polyvinyl acetal resin, and the binder will be formulated into a 10% deionized water dispersion solution.

[0032] In one specific embodiment, the thermoplastic resin includes only polyvinyl acetal resin; in other alternative embodiments, the thermoplastic resin includes polyvinyl acetal resin and other thermoplastic resins.

[0033] Exemplarily, other thermoplastic resins include one or more of ethylene-vinyl acetate copolymer resin, ethylene-acrylic acid copolymer resin, polyurethane resin, polyvinyl alcohol resin, polyester resin, and methacrylic acid copolymer resin; the ratio of polyvinyl acetal resin and other thermoplastic resins is not limited here, as long as the above-mentioned conductivity ≤100μS / cm is met.

[0034] In a specific embodiment, from the viewpoint of minimizing ash content or completely avoiding ash content, the binder is formulated into a 10% by mass deionized water solution or dispersion solution, and its conductivity is ≤50 μS / cm at 25°C.

[0035] In a specific embodiment, from the viewpoint of minimizing the ash or metal content, the binder is formulated into a 10% by mass ethanol solution, and at 25°C, the conductivity of the 10% ethanol solution thereof is ≤50μS / cm; preferably, the conductivity of the 10% ethanol solution thereof is ≤30μS / cm.

[0036] The above method for controlling the conductivity of the deionized water solution or dispersed solution and the ethanol solution may be one or more methods of washing, centrifugation, filtration, extraction and fractionation when producing the binder for ceramic capacitors. As a washing method, the washing liquid temperature is 20-80°C, and the washing times are not less than 5 times; more preferably, the washing liquid temperature is 20-60°C, and the washing times are 7-10 times; further preferably, the washing liquid temperature is 30-60°C, and the washing times are 7-10 times; the washing liquid is a solvent that is incompatible with the binder, such as water, methanol, ethanol, n-propanol, isopropanol, butanol, acetone, butanone, N,N-dimethylformamide, dimethyl sulfoxide, tetrahydrofuran, n-hexane, ethyl acetate, etc., and only one washing liquid can be used, or two or more washing liquids can be used in combination. For binders that are insoluble in water, water or a mixed solvent of water and ethanol is more preferably used, and the ratio of water to ethanol in the mixed solvent of water and ethanol is 100: (0-65). For binders that are soluble in water, one or more of methanol, ethanol, n-propanol, and isopropanol are more preferably used. As a centrifugation method, a binder is added to the above-mentioned washing liquid and then dehydrated by high-speed centrifugation. The amount of washing liquid added can be added by technicians according to the specific situation; the high-speed centrifugation speed is not less than 300 rpm, the high-speed centrifugation time is not less than 2 minutes, and the number of centrifugation is not less than 1 time; more preferably, the high-speed centrifugation speed is not less than 600 rpm, the high-speed centrifugation time is not less than 3 minutes, and the number of centrifugation is not less than 3 times; further preferably, the high-speed centrifugation speed is not less than 800 rpm, the high-speed centrifugation time is not less than 4 minutes, and the number of centrifugation is not less than 3 times.

[0037] In order to effectively prevent the binder from generating gel micelles during the sol process, the viscosity of a 30% ethanol solution of the binder at 25°C is ≤70,000 mPa·s; more preferably, the viscosity of a 30% ethanol solution of the binder at 25°C is ≤50,000 mPa·s; further preferably, the viscosity of a 30% ethanol solution of the binder at 25°C is ≤30,000 mPa·s.

[0038] In order to effectively avoid the misalignment of devices, components, connectors, etc. bonded by the adhesive, the glass transition temperature of the adhesive is ≥40°C, more preferably the glass transition temperature of the adhesive is ≥55°C, and further preferably the glass transition temperature of the adhesive is ≥60°C.

[0039] In order to effectively avoid the occurrence of insufficient debinding of the binder, the maximum thermal decomposition temperature of the binder is ≤450°C; more preferably, the maximum thermal decomposition temperature of the binder is ≤430°C, and further preferably, the maximum thermal decomposition temperature of the binder is ≤420°C.

[0040] The polyvinyl acetal resin is prepared by condensing polyvinyl alcohol and aldehyde compounds under acid catalysis. The viscosity of a 4% deionized water solution of polyvinyl alcohol (mass fraction) is preferably 3-40 mPa·s, more preferably 3-10 mPa·s, and further preferably 5-10 mPa·s. Among them, the aldehyde compound preferably has 2 to 8 carbon atoms and 1 to 3 oxygen atoms, and can be listed as: acetaldehyde, glyoxal, glyoxylic acid, chloroacetaldehyde, propionaldehyde, methylglyoxal, acrolein, 2,3-epoxypropionaldehyde, n-butyraldehyde, isobutyraldehyde, crotonaldehyde, ethyl glyoxylate, n-valeraldehyde, glutaraldehyde, 2-methylbutyraldehyde, 3-methylbutyraldehyde, n-hexanal, 2-methylvaleraldehyde, 3-methyl-1-valeraldehyde, 3,3-dimethylbutyraldehyde, n-heptylaldehyde, 2-isopropylbutyraldehyde, benzaldehyde, n-octanal, vanillin, 2-carboxybenzaldehyde, etc., preferably acetaldehyde, propionaldehyde, n-butyraldehyde, isobutyraldehyde, n-valeraldehyde, glutaraldehyde, more preferably acetaldehyde, n-butyraldehyde, n-valeraldehyde, the above aldehyde compounds can be used alone or in combination of two or more. The acidic catalyst may be an inorganic acid, an organic acid, or a mixture of an inorganic acid and an organic acid, and may include: hydrochloric acid, sulfuric acid, nitric acid, formic acid, oxalic acid, benzenesulfonic acid, preferably hydrochloric acid, formic acid, oxalic acid, benzenesulfonic acid. The above acids may be used alone or in combination of two or more.

[0041] In the process of synthesizing the polyvinyl acetal resin, an antioxidant needs to be added; preferably, the antioxidant includes a mixture of one or two of a phenolic antioxidant and a phosphate antioxidant. In an alternative embodiment, no antioxidant is added to the polyvinyl acetal resin during the condensation process, but the antioxidant is mixed with the polyvinyl acetal resin to form a binder. In another alternative embodiment, an antioxidant is added during the synthesis or preparation of the polyvinyl acetal resin, and the synthesized polyvinyl acetal resin and the antioxidant are mixed to form a binder.

[0042] Exemplary phenolic antioxidants include: β-(4-hydroxyphenyl-3,5-di-tert-butyl) propionate n-octadecanol ester, tetrakis[methyl-β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] pentaerythritol ester, 2,6-di-tert-butyl-4-methylphenol, β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate isooctyl ester, N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl) hexanediamine, 1,2-bis(3,5-di-tert-butyl-4-hydroxy-phenylpropionic acid) hydrazine, triethylene glycol bis-β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate, 3,9-bis[2-[3-(3-tert-butyl-4-hydroxyphenyl) propionate] [hydroxy-5-methylphenyl)-propionyloxy]-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane, butylated hydroxyanisole, 4,4'-thiobis(6-tert-butyl-3-methylphenol), 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, 6-(4-hydroxy-3,5-di-tert-butylphenylamino)-2,4-di-n-octylthio-1,3,5-triazine, butylated product of p-cresol and dicyclopentadiene, 2,2-oxalylamino-bis[ethyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)]propionate, 4,4'-methylenebis(2,6-di-tert-butylphenol), etc. The above antioxidants may be used alone or in combination of two or more.

[0043] The above-mentioned phosphate antioxidants include: tri(dipropylene glycol) phosphite, pentaerythritol diisodecyl diphosphite, triisodecyl phosphite, tridodecyl phosphite, tri(2, 4-di-tert-butylphenyl) phosphite, dioctadecyl pentaerythritol diphosphite, bis(2,4-di-tert-butylphenyl) pentaerythritol bis diphosphite, 3,5-di-tert-butyl-4-hydroxybenzyl diethylphosphonate, diethyl bis[(3.5 di-tert-butyl-4-hydroxybenzyl]methyl] phosphate calcium salt, 4,4'-isopropyl diphenyl C12-15-ol phosphite, 4,4'-butylene bis-(3-methyl-6-tert-butylphenyl)-tetra(tridecyl) diphosphite, bis(2,4-dicumylphenyl) pentaerythritol diphosphite, diphenyl monoisodecyl phosphite, diphenyl isooctyl phosphite, poly(dipropylene glycol) phenyl phosphite, etc. The above antioxidants can be used alone or in combination of two or more.

[0044] The mass content of the hydroxyl structural unit of the polyvinyl acetal resin is preferably 13 to 26%, more preferably 15 to 22%, and even more preferably 17 to 21%.

[0045] The following examples are provided to illustrate the present invention in more detail, but the present invention is not limited to these examples.

[0046] Example 1

[0047] 100 parts by weight of polyvinyl alcohol (4% aqueous solution viscosity 11 mPa∙s), 50 parts by weight of 33% concentrated hydrochloric acid, 60 parts by weight of butyraldehyde, and 0.35 parts by weight of an antioxidant are mixed and then subjected to a condensation reaction.

[0048] After the reaction is completed, alkali is added for neutralization, and then the reactants are washed. Deionized water is used as the washing liquid, the washing temperature is 20 ° C, the washing number is 8 times, and the washing time is 40 min each time. After each washing, ordinary dehydration or centrifugal dehydration operation can be performed. Ordinary dehydration is to discharge water naturally, and centrifugal dehydration is to discharge water through a centrifuge. Parameters such as centrifugal speed, centrifugal time, and centrifugal number are controllable. In this embodiment, ordinary dehydration is selected, and the dehydrated product is finally dried. In the exemplary embodiment, the antioxidant selects a phenolic antioxidant, for example, β-(4-hydroxyphenyl-3,5-di-tert-butyl) propionic acid n-octadecyl alcohol ester is used, and the weight fraction of the antioxidant in the polyvinyl alcohol acetal resin is less than 1%, and the technician can adjust it according to the actual situation to obtain a binder.

[0049] Examples 2 to 12 and Comparative Example 1

[0050] Polyvinyl alcohol, acid catalyst, and aldehyde compound are measured according to Table 1, and 0.35 parts by weight of antioxidant are added. The above raw materials are mixed and then subjected to condensation reaction.

[0051] After the reaction is completed, alkali is added for neutralization, and then the reactant is washed. The type of washing liquid, washing temperature, and washing times are carried out according to Table 1, and each washing time is 40 min. After each washing, ordinary dehydration or centrifugal dehydration operation can be carried out. Ordinary dehydration means that water is naturally discharged. The centrifugal speed, centrifugal time, and centrifugal times of the centrifugal operation are carried out according to Table 1. Finally, the dehydrated product is dried to obtain a binder.

[0052] Among them, Examples 6-8 directly use the centrifugal method to control the conductivity of the binder; Examples 9-12 first use the washing method to wash the binder, and after each washing, use the ordinary dehydration method to dehydrate it, and then use the centrifugal method to control the conductivity of the binder again.

[0053] Polyvinyl alcohol 4% aqueous solution (mass fraction), viscosity test, refer to GB / T 12010.2-2010 "Plastics. Polyvinyl alcohol materials (PVAL). Part 2: Performance determination" viscosity test method for testing.

[0054] For polyvinyl acetal resin, the hydroxyl content shall be tested according to the hydroxyl test method in Appendix A of HG / T 6047-2022 “Polyvinyl butyral resin for film”.

[0055] Binder, viscosity test, the binder was dissolved in ethanol at a concentration of 10% and 30%, and the dissolved solution was tested according to the method of GB / T 12008.7-2010 "Plastic polyether polyols Part 7: Determination of viscosity".

[0056] Binder, glass transition temperature test, refer to GB / T 19466.2-2004 "Plastics Differential Scanning Calorimetry (DSC) Part 2; Determination of Glass Transition Temperature" method for testing.

[0057] Binder, maximum thermal decomposition temperature test, refer to GB / T 31850-2015 "Determination of thermal decomposition temperature of non-metallic sealing materials" method for testing.

[0058] Adhesive, yellowing test, spread the adhesive on a 10cm×10cm clean glass sheet (glass sheet meets GB11614-2022 standard, thickness 2mm, b value <0.5), put it in an oven, bake at 180℃ for 1h, take it out and cool it to room temperature, test the b value with a colorimeter, measure 5 times and take the average value. The b value is: the b value in the color space for non-self-illumination specified by the International Commission on Illumination in 1976 (i.e. CIE1976Lab) represents the b value of the Lab color chromaticity index; specifically, the b value represents the range from blue to yellow, and the value range is generally -60 to 60, where negative values ​​represent blue and positive values ​​represent yellow.

[0059] Binder, conductivity test, the binder was prepared into 10% aqueous dispersion and 10% ethanol solution, heated to 50℃, maintained for 1h, and then cooled to 25℃. After the aqueous dispersion sample filtered the binder, the filtrate was used as the sample to be tested, and the 10% ethanol solution can be tested directly. The test solution was tested according to GB / T 11007-2008 "Conductivity Meter Test Method".

[0060] Binder, ash test, refer to GB / T 9345.1-2008 "Plastics. Determination of ash content. Part 1: General method" method for testing.

[0061] Binder, metal element content test, refer to GB / T 41945-2022 "Determination of metal content of raw rubber and vulcanized rubber by inductively coupled plasma optical emission spectrometer (ICP-OES)" method for testing.

[0062] Ceramic capacitor (MLCC) electrical performance evaluation

[0063] Preparation of MLCC capacitors: The binders of the embodiments and comparative examples are respectively formulated into glue with a solid content of 20% (mass fraction), and the glue is mixed with ceramic powder to form a ceramic slurry. For example, the ceramic powder is the ceramic powder used in the prior art to prepare MLCC. The ceramic slurry is coated on a PET release film and dried to obtain a ceramic green sheet. Screen printing is performed on the ceramic green sheet, and a conductive paste containing nickel is printed on it to form a conductive film for the internal electrode. Multiple ceramic green sheets with conductive films are stacked and crimped to obtain an unprocessed laminate. Next, the unprocessed laminate is sintered. Specifically, first, heat to 500°C in a nitrogen atmosphere to burn the adhesive. Then, sinter at 1250°C for 3 hours. Then, the external electrode slurry is applied to the sintered ceramic body and sintered at 1250°C for 3 hours. The end is then electroplated to obtain a stacked ceramic capacitor.

[0064] MLCC insulation resistance test: The MLCC prepared above is heat treated at 140~150℃ for 1 hour. After the heat treatment, it is placed for 24±2 hours and tested using an insulation resistance tester. Connect the test leads of the insulation resistance tester to the two terminals of the MLCC, set a suitable voltage, and measure. If the measured resistance value IR≥10000MΩ, it is judged to be qualified; if the resistance value is lower than the judgment value, it means that there may be leakage inside the MLCC and it is judged to be unqualified.

[0065] The details and results are shown in Table 1. By comparing Examples 1 to 12 with Comparative Example 1, when the conductivity of the binder is controlled within the above range, the ash content and metal element content of the binder can be well controlled.

[0066] The above description is only an exemplary embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

[0067] Table 1 Specific embodiments of the present invention

[0068] (Continued) Table 1 Specific embodiments of the present invention

Claims

1. A ceramic binder, characterized in that: The binder is used in a ceramic manufacturing process, the binder comprises a thermoplastic resin, and the thermoplastic resin comprises at least a polyvinyl acetal resin; The binder is prepared into a deionized water solution or a dispersed solution with a mass fraction of 10%, and its conductivity is ≤100μS / cm at 25°C.

2. A ceramic binder according to claim 1, characterized in that: The binder is prepared into an ethanol solution with a mass fraction of 10%, and the conductivity of the 10% ethanol solution is ≤50μS / cm at 25°C.

3. A ceramic binder according to claim 1, characterized in that: The binder is baked at 180° C. for 1 hour, and its b value is ≤5.

4. A ceramic binder according to claim 1 or 2, characterized in that: The binder is prepared into an ethanol solution with a mass fraction of 10%, and the viscosity of the 10% ethanol solution is ≤500mPa·s at 25°C.

5. A ceramic binder according to claim 1 or 2, characterized in that: The binder is prepared into an ethanol solution with a mass fraction of 30%, and the viscosity of the 30% ethanol solution is ≤70000 mPa·s at 25°C.

6. A ceramic binder according to any one of claims 1 to 3, characterized in that: The glass transition temperature of the binder is ≥40°C.

7. A ceramic binder according to any one of claims 1 to 3, characterized in that: The maximum thermal decomposition temperature of the binder is ≤450°C.

8. A ceramic binder according to any one of claims 1 to 3, characterized in that: The polyvinyl acetal resin is prepared by condensing polyvinyl alcohol and aldehyde compounds under acid catalysis conditions.

9. The ceramic binder according to claim 8, characterized in that: The molecular formula of the aldehyde compound contains 2-8 carbon atoms and 1-3 oxygen atoms; the mass content of hydroxyl groups in the polyvinyl acetal resin is 13%-26%.

10. An electronic ceramic component, characterized in that: The ceramic binder according to any one of claims 1 to 9 is used for preparation.

11. An electronic ceramic component according to claim 10, characterized in that: The electronic ceramic component comprises a ceramic capacitor or a ceramic substrate.

Citation Information

Patent Citations

  • Preparation method of photovoltaic special polyvinyl butyral (PVB) resin

    CN104059189A

  • Continuous preparation method for catalytically synthesizing polyvinyl butyral resin through organic acid

    CN105001357A

  • Binder for formation of ceramic or for use in conductive paste, and use of same

    CN106232636A

  • Heat-resistant low-viscosity polyvinyl acetal resin and preparation method thereof

    CN110903421A

  • Synthesis process of low-volatile and odorless polyvinyl butyral resin powder

    CN116082540A

Cited By

  • Water-based adhesive for nano ceramic forming as well as preparation method and application of water-based adhesive

    CN121159760A

  • Water-based adhesive for nano-ceramic molding and preparation method and application thereof

    CN121159760B

  • Nitride glass sintering aid as well as preparation method and application thereof

    CN121651675A