Method for resource utilization of ferroniobium through dressing and smelting

Through the process of combining ferroniobium coflotation and improved chlorination calcination, the efficient separation of ferroniobium concentrate is solved by using composite chlorination agent and chlorination enhancer, which has long process and low efficiency in the existing ferroniobium smelting process. The problem is that efficient recycling and high-grade extraction of niobium and iron resources are achieved.

CN119040618APending Publication Date: 2024-11-29CENT SOUTH UNIV

Patent Information

Application Number
CN202411150895.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing niobium concentrate smelting process has problems such as long process flow, low recycling efficiency, low metal resource recovery rate and large waste slag, making it difficult to achieve industrial application.

Method used

Using a process of combining niobium coflotation and improved chlorination calcination, the combined use of composite chlorination agent, chlorination enhancer and carbonaceous reducing agent is used to control the condensation temperature and recover niobium and iron chlorides to achieve niobium Efficient separation and recycling of iron.

Benefits of technology

It has achieved the characteristics of short process flow, high separation efficiency, small waste residue, high niobium recovery rate and high grade, and improved the smelting and recycling efficiency of niobium and iron resources, and is suitable for efficient extraction of Baiyun Obo niobium ore.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a method for resource utilization of ferroniobium through dressing and smelting, and belongs to the technical field of dressing and smelting. Carrying out ferroniobium co-flotation on the ferroniobium mineral to obtain ferroniobium bulk concentrate; the ferroniobium bulk concentrate is mixed with a composite chlorinating agent (including calcium chloride and ammonium chloride), a chlorination enhancer and a carbonaceous reducing agent for chloridizing roasting, and chloridized products volatilized in the chloridizing roasting process are subjected to gradient separation and recovery by controlling the condensation temperature, so that ferrum chloride and niobium chloride are obtained respectively. According to the method, the niobium and the iron are separated and recycled through the technology combining ferroniobium co-enrichment and chloridizing roasting, the method has the advantages of being short in technological process, simple, efficient in separation, small in waste residue amount, high in niobium recovery rate, high in grade and the like, and efficient smelting recovery and utilization of Bayan obo niobium and iron resources can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for selecting and smelting ferroniobium for resource utilization, and in particular to a method for separating and recovering niobium and iron by co-enrichment of ferroniobium and chlorination roasting, belonging to the technical field of niobium and iron resource selection and smelting. Background Art

[0002] Niobium has a series of excellent properties such as excellent ductility, conductivity, acid resistance and processing performance. It is a metal element with extremely wide application fields. It has an irreplaceable position in steel, superconductivity, electronics, medical treatment, nuclear industry, special alloys and cutting-edge technology.

[0004] At present, the methods for extracting niobium at home and abroad are mainly divided into alkali decomposition method, acid decomposition method and chlorination roasting method, etc. These technologies have certain advantages and disadvantages:

[0005] Alkali decomposition mainly refers to alkali melting decomposition and alkaline hydrothermal decomposition. Alkali melting decomposition is the earliest method used in the hydrometallurgical industry of niobium resources. Its main disadvantages are low niobium yield (<80%), large alkali consumption and complicated process. When treating niobium ore by alkaline hydrothermal method, the reaction temperature is much lower than that of alkali melting decomposition, and the alkali consumption is greatly reduced, which is about 1 / 6 of that of alkali melting method. However, the process is operated under pressure, which is difficult to operate, resulting in its failure to achieve industrialization.

[0006] The acid decomposition method mainly refers to the sulfuric acid low-temperature roasting method and the hydrofluoric acid decomposition method. The sulfuric acid low-temperature roasting method has a high metal decomposition rate and can recover most of the valuable metal components in the niobium ore, but it can only be used for easily decomposed niobium ores, with a narrow range of raw material applications, low product purity, long operation process, and large sulfuric acid consumption in the process. It is rarely used in actual production. The main advantages of the hydrofluoric acid decomposition method are low energy consumption and simple process. The decomposition rate of high niobium content concentrate can reach 98% to 99%. Its main disadvantages are the low decomposition rate of low-grade niobium concentrate, large amount of waste slag, large consumption of hydrofluoric acid in the process, and due to the high toxicity and strong corrosiveness of hydrofluoric acid, this method has high requirements on equipment materials, good ventilation devices and recovery systems, and high production costs.

[0007] Chlorination roasting is a relatively common and industrially valuable method for extracting niobium. It can be used to process complex niobium concentrates, but the existing technology still has certain defects. For example, the traditional solid chlorinating agent has poor chlorine supply performance, resulting in a low metal resource recovery rate; the enhanced chlorine supply measures taken are prone to secondary pollution during implementation.

[0008] In summary, the current process of extracting niobium from niobium ferroconcentrate faces many difficulties. The industry urgently needs to develop a new niobium ferroconcentrate smelting process with short process and high efficiency. Summary of the invention

[0009] In order to solve the technical problems of long process flow and low recovery efficiency in the existing technology of smelting and recovering niobium, the purpose of the present invention is to provide a method for beneficiating and smelting ferroniobium for resource utilization. The method utilizes a process combining niobium and iron co-enrichment and chlorination roasting to separate and recover niobium and iron. The method has the characteristics of short process flow, simple method, efficient separation, small amount of waste slag, high niobium recovery rate, high grade, etc., and can realize the efficient smelting, recovery and utilization of Bayan Obo niobium and iron resources.

[0010] In order to achieve the above technical objectives, the present invention provides a method for beneficiating and smelting ferroniobium for resource utilization, the method comprising the following steps:

[0011] 1) co-floating ferroniobium ore to obtain an iron-niobium mixed concentrate;

[0012] 2) Mixing the ferroniobium mixed concentrate with a composite chlorinating agent, a chlorination enhancer and a carbonaceous reducing agent for chlorination roasting, and volatilizing chlorination products during the chlorination roasting process by controlling the condensation temperature for stepwise separation and recovery to obtain iron chloride and niobium chloride respectively; the composite chlorinating agent includes calcium chloride and ammonium chloride.

[0013] The technical solution of the present invention first realizes the co-enrichment of iron and niobium in ferroniobium ore by co-flotation of niobium and iron, and then uses the chlorination method to decompose the ferroniobium mixed concentrate. The iron-niobium mixed concentrate reacts chemically with the chlorinating agent under high temperature conditions, mainly converting niobium compounds and iron compounds into niobium chloride and iron chloride, and then separating them by using the volatility characteristics of the two. The main chemical equations of niobium minerals in the chlorination roasting process are: Nb2O5+C+Cl2→NbCl5+CO; Nb2O5+C+Cl2→NbCl5+CO2; iron minerals mainly generate ferric chloride in the chlorination roasting process, and the boiling point of NbCl5 is 254°C, and the boiling point of FeCl3 is 315°C. According to the difference in boiling points, the conditions such as the condenser temperature can be controlled to separately collect chlorides such as iron chloride and niobium, thereby realizing the resource recovery of niobium and iron in ferroniobium ore.

[0014] The key to the technical solution of the present invention is to adopt an improved chlorination roasting method. On the one hand, a special composite chlorinating agent is used. The combination of calcium chloride and ammonium chloride produces a synergistic effect to improve the efficiency of chlorination roasting. Calcium chloride provides Cl -On the one hand, ammonium chloride is easily decomposed when heated to produce NH3 and Cl2, which helps to improve the kinetics of the chlorination reaction and improve the chlorination efficiency, which is better than using a single chlorinating agent; on the other hand, a chlorination enhancer is used, which can promote the decomposition of calcium chloride to produce chlorine gas and achieve secondary chlorination; on the third hand, a carbonaceous reducing agent is introduced. Since the chlorination roasting system contains a large amount of oxygen, the presence of oxygen will increase the difficulty of chlorination, and in the presence of a carbonaceous reducing agent, it can combine with active oxygen, which is beneficial to the combination of metals such as niobium and iron with chlorine, thereby reducing the starting temperature of chlorination and improving the chlorination efficiency.

[0015] As a preferred solution, the composite chlorinating agent is composed of calcium chloride and ammonium chloride in a mass ratio of (0.2-0.5):1. If the mass ratio of calcium chloride and ammonium chloride is too high, the chlorination reaction will be incomplete, the roasting temperature will be required to be higher, and energy consumption will be increased. If the mass ratio of calcium chloride and ammonium chloride is too low, the HCl concentration in the reaction system will be high, causing corrosion and reducing the utilization rate of the chlorinating agent. As a preferred solution, CaCl2 has the characteristics of stable chlorine supply, and ammonium chloride will decompose into NH3 and Cl2 during the roasting process, which can avoid the introduction of additional metal impurities.

[0016] As a preferred solution, the chlorination enhancer includes ferrous sulfate. Ferrous sulfate decomposes at a high temperature above 700°C to produce SO2 and O2, which promotes the decomposition of CaCl2 to generate Cl2, thereby performing secondary chlorination.

[0017] As a preferred solution, the carbonaceous reducing agent includes at least one of charcoal and petroleum coke. As a preferred solution, it is difficult to directly use minerals for chlorination reaction, so the chlorination reaction roasting needs to be carried out under the action of a reducing agent, which combines with oxygen to reduce the oxygen activity, which is conducive to the combination of metal and chlorine, thereby reducing the chlorination starting temperature and improving the chlorination efficiency.

[0018] As a preferred solution, the mass ratio of the composite chlorinating agent, chlorination enhancer, reducing agent and ferroniobium mixed concentrate is (1-3):(0.5-1):(0.1-0.3):1. The optimization and determination of the ratio between the composite chlorinating agent, chlorination enhancer, reducing agent and ferroniobium mixed concentrate takes into account factors such as chemical reaction equilibrium, reaction thermodynamics and kinetics, and environmental safety. If the ratio of the composite chlorinating agent is too high, the chlorinating agent is wasted, the cost is increased, excessive chlorination is caused, unnecessary by-products are generated, and equipment corrosion problems will occur; if the ratio of the composite chlorinating agent is too low, the chlorination reaction will be insufficient, affecting the metal yield. If the ratio of the chlorination enhancer is too high, excessive chlorination will result in increased operating costs. If the ratio of the chlorination enhancer is too low, the chlorination efficiency will be reduced. If the ratio of the reducing agent is too high, the reducing atmosphere generated is too strong, affecting the stability of certain metal chlorides; causing undesirable reduction reactions and generating impurities. If the ratio of the reducing agent is too low, sufficient reducing atmosphere cannot be provided, affecting the chlorination effect of difficult-to-chlorinate metals. If the proportion of niobium-iron mixed concentrate is too high or too low, it will directly affect the material input cost and metal output, and may also affect the uniformity of the reaction and the fluidity of the material.

[0019] As a preferred solution, the chlorination roasting conditions are: a heating rate of 10 to 25°C / min, and roasting for 30 to 45 minutes at a temperature of 700 to 900°C. Within the preferred roasting temperature range, as the roasting temperature increases, the overall chlorination volatilization rate of iron and niobium gradually increases, and sufficient volatilization time ensures sufficient chlorination volatilization of iron and niobium. Further increasing the chlorination roasting temperature does not significantly increase the chlorination volatilization efficiency of niobium and iron.

[0020] As a preferred solution, the process of niobium-iron co-flotation is as follows: the pH of the niobium-iron mineral slurry is adjusted to alkaline, a metal organic complex is used as a co-flotation collector for iron minerals and niobium minerals, and a gangue mineral inhibitor is used at the same time to perform flotation separation to obtain an iron-niobium mixed concentrate; the metal organic complex is formed by coordination between a divalent or higher metal ion and a hydroxamic acid organic ligand.

[0021] As a preferred solution, the pH of the ferroniobium mineral slurry is adjusted to 8.5-10.5. The pH is adjusted using alkaline compounds such as Na2CO3 or NaOH. Under the preferred pH conditions, the Pb 2+ 、PbOH + 、Pb(OH) 2(aq) It reacts with BHA anionic ligands to form one or several metal ion complexes, which have properties similar to lead ions and colloidal properties. Its colloidal structure carries positive charges and can be adsorbed on the mineral surface through electrostatic effects. The surface potential of the mineral changes from negative to positive, thus enhancing the adsorption and binding ability of the collector on the mineral surface.

[0022] As a preferred solution, the metal ion in the metal organic complex is lead ion, and the organic ligand is at least one of octyl hydroxamic acid, benzohydroxamic acid, and oleic acid. The lead ion and the hydroxamic acid ligand are assembled to form micelles with a specific structure and specific capture ability, which have a highly selective action on Nb-O bonds, and the hydroxamic acid group has a high selectivity on the active Fe on the surface of the iron mineral. 3+ , Fe 2+ It has a particularly strong binding ability and can chelate to form extremely stable quaternary or quinary chelates, which can perform surface hydrophobic modification on iron minerals, which is beneficial to the co-floatation of iron and niobium.

[0023] As a preferred solution, the gangue mineral inhibitor includes at least one of water glass, sodium fluorosilicate, and sodium carboxymethyl cellulose. The preferred gangue mineral inhibitor is mainly used to inhibit gangue minerals such as SiO2.

[0024] The iron-niobium mixed concentrate of the present invention is dried and then subjected to chlorination roasting, the drying temperature is 105° C., and the drying time is controlled between 1.5 and 2.0 hours.

[0025] In the present invention, inert gas such as argon is introduced as protective gas during the chlorination roasting process, and the flowing inert gas is used as carrier gas, which is conducive to the volatilized metal chloride entering the condensation collection device. The flow rate of argon is generally 50 mL min -1 , the intake pressure is 0.5~2MPa.

[0026] The scraper is installed inside the condenser of the present invention, and can be rotated in the condenser to scrape out condensate.

[0027] Compared with the existing technology for extracting niobium, the technical solution of the present invention has beneficial technical effects:

[0028] 1) The present invention uses a reinforced chlorination roasting system combining a composite chlorinating agent and a chlorination enhancer, and the niobium and iron resource recovery rate is high and the grade is high.

[0029] 2) According to the difference in boiling points of metal chlorides, the present invention controls the temperature of the condenser to separate and recover chlorides such as iron and niobium in stages, thereby achieving efficient resource recovery of niobium and iron in the Bayan Obo mine.

[0030] 3) In view of the advantages of the chlorination roasting method and the complex composition of the Bayan Obo niobium ore, the present invention uses a composite chlorination agent to strengthen the roasting on the basis of achieving efficient enrichment of iron and niobium based on niobium-iron co-enrichment flotation, so as to achieve efficient extraction of niobium-iron resources in the Bayan Obo mine, transforming resource advantages into technical advantages, which is conducive to promoting the rational development and efficient utilization of niobium resources. DETAILED DESCRIPTION

[0031] The following specific examples are intended to further illustrate the present invention rather than to limit the scope of protection of the claims.

[0032] The niobium iron concentrate after further flotation of the rare earth tailings of the Bayan Obo Main East Mine was taken as the experimental research object. The following Table 1 shows the main chemical composition of the niobium iron concentrate. Its composition is complex, mainly Fe2O3 and SiO2, and the Nb2O5 grade is 2.09%.

[0033] Table 1 Main chemical composition of niobium iron concentrate

[0034]

[0035] Example 1

[0036] The overall flotation process is: one roughing, one sweeping and four fines. The roughing process is mainly to flotation pulp pH 9.5, use water glass to inhibit gangue minerals, pre-mix the lead solution and benzohydroxamic acid in a molar ratio of 2:1, and the overall roughing agent dosage is 800g / t, which is then poured into the pulp for overall flotation separation. The flotation concentrate is dried at 105℃ for 1h. Weigh 500g of the concentrate powder that has been dried and ground to -200 mesh, and mix the materials evenly according to the mass ratio of composite chlorinating agent: enhancer: reducing agent: niobium iron concentrate = 1.5:0.75:0.2:1. The composite chlorinating agent uses CaCl2 and NH4Cl, where the mass ratio of CaCl2:NH4Cl is 0.25:1. The enhancer uses FeSO4·7H2O. The reducing agent uses charcoal. The mixed sample was placed in a crucible and heated from room temperature to the set temperature at 25°C / min in an argon atmosphere of a muffle furnace. The roasting temperatures were set to 700°C, 800°C, 900°C and 1000°C, respectively, and the roasting time was set to 30 minutes. The gas phase products volatilized during the roasting process were passed into a three-stage condenser, and the condenser temperatures were set to 315°C, 254°C and 80°C, respectively. The condensation product recovery data is shown in Table 2 below.

[0037] Table 2 Effect of calcination temperature on Nb and Fe metal recovery

[0038]

[0039] Example 2

[0040] The flotation process is referred to Example 1. Weigh 500g of the concentrate powder that has been dried and ground to -200 mesh, and mix the materials evenly according to the mass ratio of composite chlorinating agent: strengthening agent: reducing agent: niobium iron concentrate = 1.5:0.75:0.2:1. The composite chlorinating agent uses CaCl2 and NH4Cl, wherein the mass ratio of CaCl2:NH4Cl is 0.25:1. The strengthening agent uses FeSO4·7H2O. The reducing agent uses charcoal. The mixed sample is placed in a crucible, and the temperature is raised from room temperature to the set temperature at 25°C / min in the argon atmosphere of the muffle furnace. The roasting temperature is set to 900°C, and the roasting time is set to 8min, 15min, 30min and 45min respectively. The gas phase products volatilized during the roasting process are passed into a three-stage condenser, and the condenser temperatures are set to 315°C, 254°C and 80°C respectively. The condensation product recovery data is shown in Table 3 below.

[0041] Table 3 Effect of calcination time on Nb and Fe metal recovery

[0042]

[0043] Example 3

[0044] The flotation process is referred to Example 1. Weigh 500g of the concentrate powder that has been dried and ground to -200 mesh, and mix the composite chlorinating agent, the strengthening agent, the reducing agent and the niobium iron concentrate evenly according to a certain proportion. The composite chlorinating agent uses CaCl2 and NH4Cl, and the mass ratio of the composite chlorinating agent: niobium iron concentrate is controlled at 0.5:1, 1:1, 1.5:1, 2:1 and 2.5:1, wherein the mass ratio of CaCl2: NH4Cl is 0.25:1. The strengthening agent uses FeSO4·7H2O, and the mass ratio of the strengthening agent: niobium iron concentrate is 0.75:1. The reducing agent uses charcoal, and the mass ratio of the reducing agent: niobium iron concentrate is 0.2:1. The mixed sample was placed in a crucible, and the temperature was raised from room temperature to the set temperature at 25°C / min in an argon atmosphere of a muffle furnace. The roasting temperature was set to 900°C, and the roasting time was set to 30 minutes. The gas phase product volatilized during the roasting process was passed into a three-stage condenser, and the condenser temperatures were set to 315°C, 254°C, and 80°C, respectively. The condensation product recovery data is shown in Table 4 below.

[0045] Table 4 Effect of chlorinating agent addition on Nb and Fe metal recovery

[0046]

[0047] Example 4

[0048] The flotation process is referred to Example 1. Weigh 500g of the concentrate powder that has been dried and ground to -200 mesh, and mix the materials evenly according to the mass ratio of chlorinating agent: strengthening agent: reducing agent: niobium iron concentrate = 1.5:0.75:0.2:1. The chlorinating agents used are: single CaCl2, single NH4Cl and composite chlorinating agent. The composite chlorinating agent uses CaCl2 and NH4Cl, where the mass ratio of CaCl2:NH4Cl is 0.25:1. The strengthening agent uses FeSO4·7H2O. The reducing agent uses charcoal. The mixed sample is placed in a crucible, and the temperature is raised from room temperature to the set temperature at 25℃ / min in the argon atmosphere of the muffle furnace. The roasting temperature is set to 900℃, the roasting time is set to 30min, and the gas phase products volatilized during the roasting process are passed into a three-stage condenser, and the condenser temperatures are set to 315℃, 254℃ and 80℃ respectively. The condensation product recovery data is shown in Table 5 below.

[0049] Table 5 Effect of single chlorinating agent and composite chlorinating agent on Nb and Fe metal recovery

[0050]

[0051] Example 5

[0052] The flotation process is as in Example 1. Weigh 500g of the dried and ground concentrate powder to -200 mesh, and mix the materials evenly according to the mass ratio of chlorinating agent: reducing agent: niobium iron concentrate = 1.5:0.2:1. The composite chlorinating agent is CaCl2 and NH4Cl, wherein the mass ratio of CaCl2: NH4Cl is 0.25:1. The reducing agent is charcoal. One group of materials is added with a reinforcing agent, FeSO4·7H2O, and the chlorinating agent: reinforcing agent = 2:1; the other group of materials is not added with a reinforcing agent. The mixed sample is placed in a crucible, and the temperature is raised from room temperature to the set temperature at 25°C / min in the argon atmosphere of the muffle furnace. The roasting temperature is set to 900°C, the roasting time is set to 30min, and the gas phase products volatilized during the roasting process are passed into a three-stage condenser, and the condenser temperatures are set to 315°C, 254°C and 80°C respectively. The condensation product recovery data is shown in Table 6 below.

[0053] Table 6 Effect of enhancers on Nb and Fe metal recovery

[0054]

[0055] Example 6

[0056] The flotation process is referred to Example 1. Weigh 500g of the concentrate powder that has been dried and ground to -200 mesh, and mix the materials evenly according to the mass ratio of chlorinating agent: strengthening agent: niobium iron concentrate = 1.5:0.75:1. The composite chlorinating agent uses CaCl2 and NH4Cl, where the mass ratio of CaCl2: NH4Cl is 0.25:1. The strengthening agent uses FeSO4·7H2O. A group of materials is added with a reducing agent, using charcoal, and the chlorinating agent: reducing agent = 7.5:1; the other group of materials does not add a reducing agent. The mixed sample is placed in a crucible, and the temperature is raised from room temperature to the set temperature at 25℃ / min in the argon atmosphere of the muffle furnace. The roasting temperature is set to 900℃, the roasting time is set to 30min, and the gas phase products volatilized during the roasting process are passed into a three-stage condenser, and the condenser temperatures are set to 315℃, 254℃ and 80℃ respectively. The condensation product recovery data is shown in Table 6 below.

[0057] Table 6 Effect of reducing agent on Nb and Fe metal recovery

[0058]

Claims

1. A method for selecting and smelting ferroniobium for resource utilization, Features: The following steps are involved: 1) co-floating ferroniobium ore to obtain an iron-niobium mixed concentrate; 2) Mixing the ferroniobium mixed concentrate with a composite chlorinating agent, a chlorination enhancer and a carbonaceous reducing agent for chlorination roasting, and volatilizing chlorination products during the chlorination roasting process by controlling the condensation temperature for stepwise separation and recovery to obtain iron chloride and niobium chloride respectively; the composite chlorinating agent includes calcium chloride and ammonium chloride.

2. A method for selecting and smelting ferroniobium for resource utilization according to claim 1, Features: The composite chlorinating agent is composed of calcium chloride and ammonium chloride in a mass ratio of (0.2-0.5):

1.

3. The method for selecting and smelting ferroniobium for resource utilization according to claim 1, Features: The chlorination enhancer includes ferrous sulfate.

4. The method for selecting and smelting ferroniobium for resource utilization according to claim 1, Features: The carbonaceous reducing agent includes at least one of charcoal and petroleum coke.

5. A method for beneficiating and smelting ferroniobium for resource utilization according to any one of claims 1 to 4, Features: The mass ratio of the composite chlorinating agent, the chlorination enhancer, the reducing agent and the niobium-iron mixed concentrate is (1-3):(0.5-1):(0.1-0.3):

1.

6. A method for beneficiating and smelting ferroniobium for resource utilization according to any one of claims 1 to 4, Features: The conditions of the chlorination roasting are: a heating rate of 10 to 25° C. / min, a temperature of 700 to 900° C., and a roasting time of 30 to 45 minutes.

7. A method for beneficiating and smelting ferroniobium for resource utilization according to any one of claims 1 to 4, Features: The process of niobium-iron co-flotation is as follows: the pH of niobium-iron mineral slurry is adjusted to alkaline, a metal organic complex is used as a co-flotation collector for iron mineral and niobium mineral, and a gangue mineral inhibitor is used at the same time to perform flotation separation to obtain an iron-niobium mixed concentrate; the metal organic complex is formed by coordination between a divalent or higher metal ion and a hydroxamic acid organic ligand.

8. The method for selecting and smelting ferroniobium for resource utilization according to claim 7, Features: The pH of the niobium iron ore slurry is adjusted to 8.5-10.

5.

9. The method for selecting and smelting ferroniobium for resource utilization according to claim 7, Features: The metal ion in the metal organic complex is a lead ion, and the organic ligand is at least one of octyl hydroxamic acid, benzohydroxamic acid and oleic acid.

10. The method for selecting and smelting ferroniobium for resource utilization according to claim 7, Features: The gangue mineral inhibitor includes at least one of water glass, sodium fluorosilicate and sodium carboxymethyl cellulose.

Citation Information

Patent Citations

  • PROCESS FOR CLEANING SULFUR OXIDE LOADED GASES

    AT7543U1

  • Method for preparing niobium microalloy steel by using low-niobium molten iron

    CN102212736A

  • Method for co-enriching iron and niobium resources in rare earth tailings

    CN118268138A

Cited By

  • Method for recovering tantalum and niobium from waste residues and application

    CN120575047A