Preparation method of moisture absorption and sweat releasing polyester fibers

By introducing hydrophilic groups and hollow structures into polyester fibers, combined with alkali-soluble treatment, a porous structure is formed, the problem of insufficient moisture absorption and sweating performance of the fiber is solved, and the efficiency of moisture absorption and sweating performance is improved to meet the comfort level. Require and simplify production processes.

CN119041050AInactive Publication Date: 2024-11-29ZHEJIANG HENGYI PETROCHEMICAL RES INST CO LTD

Patent Information

Application Number
CN202411128429.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing fibers have shortcomings in moisture-absorbing and sweating performance, and it is difficult to meet the needs of high moisture-absorbing and high sweating at the same time, and the production process is complex or performance is limited.

Method used

By introducing hydrophilic groups and hollow structure spinning, combined with alkali-soluble treatment, we form moisture-wicking polyester fibers with porous structures, which improves the specific surface area and moisture-wicking properties of the fibers.

Benefits of technology

It significantly improves the moisture-absorbing and sweating performance of polyester fiber, achieves excellent moisture-absorbing and sweating capabilities while the fiber, meets comfort needs, and simplifies the production process.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the field of polyester fibers, and provides a preparation method of moisture-absorbing and sweat-releasing polyester fibers, aiming at the problem of poor moisture-absorbing and sweat-releasing performance of fibers, the preparation method comprises the following steps: (1) esterification reaction: adding nano diatomite into a polyester monomer, and carrying out esterification reaction to obtain an esterified product; (2) condensation polymerization: adding 5-(sodium sulfo) isotitanic acid and polyethylene glycol into the ester, and carrying out condensation polymerization to obtain modified polyester chips; (3) spinning: carrying out melt spinning on the modified polyester chips to obtain hollow polyester fibers; a chemical reagent and the hollow polyester fibers are mixed, the chemical reagent reacts to remove at least part of the nanometer diatomite, so that holes are formed in the hollow fibers, and the moisture absorption and sweat releasing polyester fibers are obtained through washing and drying. The intrinsic hydrophilic performance of a polyester material is improved by introducing a hydrophilic group, the specific surface area of the fiber is increased by combining hollow structure spinning and alkali dissolution treatment, and the moisture absorption and sweat releasing performance of the polyester fiber is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polyester fibers, and in particular to a method for preparing moisture absorbing and perspiration wicking polyester fibers. Background Art

[0002] With the development of social economy, people have higher and higher requirements for food, clothing, housing and transportation. For example, in terms of clothing, the functionality and comfort of clothing have gradually become important selection criteria. For textiles, this requires them to have functions such as moisture absorption, breathability, and perspiration. Pure cotton fabrics have excellent moisture absorption properties because they have a large number of hydrophilic groups, but sweat is not easy to discharge, making the fabric easy to adhere to the skin and cause discomfort. Conventional chemical fibers are the opposite, so the comfort level is not enough to meet people's needs. Therefore, the development of new fibers with good moisture absorption and effective perspiration has a very broad market prospect and can be used in many textiles such as sportswear, underwear, etc.

[0003] For example, patent CN104372428A discloses a moisture-absorbing and perspiration-releasing fiber, which has a cross-section similar to a "cross" structure, thereby increasing the irregularity of the fiber, and because the outer contour of the "cross" structure has four obvious grooves, the capillary effect is enhanced, so that the fiber can quickly absorb moisture and sweat from the skin surface, and diffuse and transfer to the outer layer, so that it has a strong moisture conduction and perspiration capacity. Patent CN105543996A discloses a moisture-absorbing and perspiration-releasing polyvinyl chloride fiber, including: polyvinyl chloride fiber, nylon fiber, lyocell fiber and chitin fiber, and the hygroscopicity of the polyvinyl chloride fiber is improved by limiting the proportion of each fiber.

[0004] The above-mentioned production processes and methods of moisture wicking fibers have certain limitations, that is, simply adding moisture wicking fibers or introducing hydrophilic groups (chemical modification) usually significantly improves the moisture wicking performance of the fibers, while simply increasing the specific surface area of ​​the fibers (physical modification) usually significantly improves their moisture wicking performance. Fabrics with higher comfort require fibers to have both excellent moisture wicking and sweat wicking capabilities. As mentioned above, it is of great significance to propose a method for preparing polyester fibers with a simple production process and comprehensive moisture wicking performance. Summary of the invention

[0005] In order to overcome the problem of poor moisture absorption and perspiration discharge of fibers, the present invention provides a method for preparing moisture absorption and perspiration discharge polyester fibers, introduces hydrophilic groups to improve the intrinsic hydrophilicity of polyester materials, combines hollow structure spinning and alkali dissolution treatment to increase the fiber specific surface area, and effectively improves the moisture absorption and perspiration discharge performance of the polyester fibers.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions: A method for preparing a moisture absorbing and perspiration wicking polyester fiber comprises the following steps: (1) Esterification reaction: adding nano-diatomaceous earth to polyester monomer to carry out esterification reaction to obtain esterified product; (2) polycondensation reaction: adding 5-(sodium sulfo)isotitanic acid and polyethylene glycol to the esterified product to carry out polycondensation reaction to obtain modified polyester chips; (3) Spinning: The modified polyester chips are melt-spinned to produce hollow polyester fibers; (4) Pore formation: chemical reagents are mixed with hollow polyester fibers, and the chemical reagents react to remove at least a portion of the nano-diatomaceous earth and the modified polyester matrix, so that holes are formed in the hollow fibers. The moisture-absorbing and perspiration-wicking polyester fibers are obtained by washing and drying.

[0007] The moisture absorption and perspiration wicking performance of the polyester fiber of the present invention is achieved by combining multiple principles. The moisture absorption and perspiration wicking performance of the fiber depends on both its chemical composition and physical structure. The chemical composition generally improves the hydrophilicity of the material to achieve moisture absorption, while the physical structure generally increases the specific surface area of ​​the fiber to improve the moisture wicking performance. Therefore, performing these two aspects of modification at the same time is more conducive to improving the moisture absorption and perspiration wicking performance of the polyester fiber.

[0008] The present invention first introduces a tri-monomer (5-(sodium sulfo)isotitanic acid) and a tetra-monomer (polyethylene glycol) in the polymerization stage, which can destroy the regularity of the macromolecular chain and the rigid structure of the polyester chain on the one hand, which is conducive to the penetration of water molecules; on the other hand, the polar group sulfonic acid group and the ether bond are both hydrophilic, which improves the binding ability of polyester and water, and realizes the improvement of the hygroscopicity of the polyester material from the intrinsic structure. Then in the spinning stage, the fiber specific surface area is greatly increased by spinning hollow structured special-section yarns. Finally, in the alkali dissolution stage, through the alkali solution soaking treatment of a certain concentration and time, the main component of the nano-diatomaceous earth, silicon dioxide, will react with the alkali solution to form a sodium silicate solution, and countless microporous structures will be formed at the original position of the nano-diatomaceous earth; at the same time, a small amount of hydrophilic modified polyester matrix will also be hydrolyzed in the alkali solution and dissolved into pores, and due to the presence of the hollow structure, such micropores can exist on the inner and outer wall surfaces of the fiber, further increasing its specific surface area. In addition, due to the improved hydrophilicity of the modified polyester and the cross-sectional design of the hollow structure, the fiber will form some penetrating pores after being treated with alkali solution, providing more channels for the migration of water. By utilizing the capillary effect, it can absorb sweat and moisture from the skin surface more quickly, and evaporate through diffusion and transfer to the outside.

[0009] Preferably, the particle size of the nano-diatomaceous earth is 200-800 nm; the added amount of the nano-diatomaceous earth is 0.1-5 wt % of the polyester monomer.

[0010] Preferably, the polyester monomers are terephthalic acid and ethylene glycol in a molar ratio of 1:1.1 to 1.5.

[0011] Preferably, the catalyst for the esterification reaction is one of ethylene glycol antimony, ethylene glycol titanium or tetrabutyl titanate, and the added amount is 100 to 400 ppm of the polyester monomer.

[0012] Preferably, the esterification reaction conditions are: in an inert atmosphere, first esterify at 200-220° C. for 20-50 min at normal pressure, and then esterify under pressure at 220-250° C. and 0.2-0.4 MPa for 80-180 min.

[0013] Preferably, the molar ratio of 5-(sodiosulfo)isotitanic acid to terephthalic acid is 1:20-100.

[0014] Preferably, the molecular weight of the polyethylene glycol in step (2) is 600-4000 g / mol, and the added amount is 1-5 wt % of the polyester monomer.

[0015] Preferably, the polycondensation reaction conditions are: negative compression polymerization at 260-280° C. for 0.5-2 h under vacuum conditions.

[0016] Preferably, the spinning process is as follows: the modified polyester chips are vacuum dried at 60-120°C for 10-30 hours, then added to a screw spinning machine for melt metering and spun through a hollow cross-section spinneret, wherein the spinning temperature is 260-290°C and the spinning winding speed is 2500-4000m / min.

[0017] Preferably, the chemical reagent is alkali solution, and the washing process is: the vacuum polyester fiber is washed in alkali solution at 60-90°C and 1.5-2.0 mol / L for 30-50 minutes. The alkali solution can react with the nano-diatomaceous earth particles exposed on the surface of the hollow polyester fiber to form holes, and further etch the polyester matrix to form a porous structure on the fiber surface, and then washed and dried to finally obtain a polyester fiber with moisture absorption and perspiration properties.

[0018] Therefore, the beneficial effects of the present invention are: (1) The intrinsic hydrophilicity of polyester materials is improved by introducing hydrophilic groups, and the fiber specific surface area is increased by combining hollow structure spinning and alkali dissolution treatment, which effectively improves the moisture absorption and perspiration performance of polyester fibers; (2) Due to the hollow structure of the fiber, the main component of the nano-diatomaceous earth, silicon dioxide, distributed on the fiber surface will react with the alkali solution to form partial micropores and defects on the inner and outer walls of the fiber, which is beneficial to further improve the moisture absorption and perspiration performance of the fiber; (3) Due to the improved hydrophilicity of the modified polyester and the hollow structure of the fiber, a certain amount of alkaline solution treatment can dissolve part of the polyester matrix to form penetrating pores, providing more channels and paths for the migration of water. DETAILED DESCRIPTION

[0019] The technical solution of the present invention is further described below through specific embodiments.

[0020] In the present invention, unless otherwise specified, the raw materials and equipment used can be purchased from the market or are commonly used in the art. The methods in the embodiments, unless otherwise specified, are all conventional methods in the art. Unless otherwise specified, parts are all weight parts, temperatures are expressed in ° C or at ambient temperature, and pressures are atmospheric pressure or near atmospheric pressure. There are many variations and combinations of reaction conditions (such as component concentrations, desired solvents, solvent mixtures, temperatures, pressures, and other reaction ranges) and conditions that can be used to optimize the purity and yield of the product obtained by the method, and only reasonable routine experiments will be required to optimize such method conditions.

[0021] Example A method for preparing a moisture absorbing and perspiration wicking polyester fiber comprises the following steps: (1) Esterification reaction: Add nano-diatomite with a particle size of 200-800 nm to the polyester monomer, and perform an esterification reaction under the action of a catalyst to obtain an esterified product. The amount of nano-diatomite added is 0.1-5wt% of the polyester monomer. The polyester monomer is terephthalic acid and ethylene glycol in a molar ratio of 1:1.1-1.5. The catalyst is one of ethylene glycol antimony, ethylene glycol titanium or tetrabutyl titanate, and the amount of addition is 100-400ppm of the polyester monomer. The conditions of the esterification reaction are: in a nitrogen atmosphere, first esterify at 200-220°C under normal pressure for 20-50 minutes, and then esterify under pressure at 220-250°C and 0.2-0.4MPa for 80-180 minutes.

[0022] (2) Polycondensation reaction: Add 5-(sodium sulfonated)isotitanic acid and polyethylene glycol to the esterified product to carry out polycondensation reaction to obtain modified polyester chips. The molar ratio of 5-(sodium sulfonated)isotitanic acid to terephthalic acid in step (1) is 1:20-100. The molecular weight of polyethylene glycol is 600-4000 g / mol, and the amount added is 1-5 wt% of the polyester monomer. The conditions of the polycondensation reaction are: negative compression polymerization at 260-280° C. for 0.5-2 h under vacuum conditions.

[0023] (3) Spinning: The modified polyester chips are vacuum dried at 60-120°C for 10-30 hours, then added to a screw spinning machine for melt metering and spun through a hollow cross-section spinneret to produce hollow polyester fibers. The spinning temperature is 260-290°C and the spinning winding speed is 2500-4000 m / min.

[0024] (4) Pore making: at least part of the nano-diatomaceous earth in the hollow polyester fiber is removed by washing with alkaline solution, and the moisture wicking polyester fiber is obtained by washing with water and drying. The chemical reagent is alkaline solution, and the washing process is: the vacuum polyester fiber is washed in alkaline solution at 60-90°C and a concentration of 1.5-2.0 mol / L for 30-50 minutes.

[0025] Example 1 A method for preparing a moisture absorbing and perspiration wicking polyester fiber, comprising the following steps: (1) Esterification reaction: terephthalic acid and ethylene glycol in a molar ratio of 1:1.4 are used as polyester monomers. Based on the mass of the polyester monomer, 250 ppm of catalyst ethylene glycol antimony and 2 wt % of diatomaceous earth with a particle size of 500 nm are added to the polyester monomer; under a nitrogen atmosphere, esterification is first performed at 210° C. at normal pressure for 30 min, and then at 240° C. and 0.3 MPa under pressure for 120 min to obtain an esterified product.

[0026] (2) polycondensation reaction: adding 5-(sodium sulfonated)isotitanic acid and polyethylene glycol with a molecular weight of 2000 g / mol to the esterified product, wherein the molar ratio of 5-(sodium sulfonated)isotitanic acid to terephthalic acid in step (1) is 1:50, and the amount of polyethylene glycol added is 2 wt% of the mass of the polyester monomer in step (1); performing negative compression polymerization at 278° C. for 1 h under vacuum conditions, and then stopping the reaction to obtain modified polyester, and preparing modified polyester chips by conventional methods.

[0027] (3) Spinning: The modified polyester chips were vacuum dried at 100°C for 24 hours, and then added to a screw spinning machine for melt metering and spun through a hollow cross-section spinneret, wherein the spinning temperature was 280°C and the spinning winding speed was 3000 m / min, to obtain a hollow structured modified polyester fiber.

[0028] (4) Pore formation: The polyester fiber is alkaline washed in a sodium hydroxide aqueous solution at 80°C and a concentration of 1.5 mol / L for 30 min to react with the diatomaceous earth exposed on the surface of the hollow fiber to form pores, and the polyester matrix is ​​further etched to form a porous structure on the fiber surface. The fiber is then washed with water and dried to finally obtain a moisture-absorbing and perspiration-wicking polyester fiber.

[0029] Example 2 The difference from Example 1 is that the amount of hydrophilic monomer used in step (2) is reduced.

[0030] A method for preparing a moisture absorbing and perspiration wicking polyester fiber, comprising the following steps: (1) Esterification reaction: terephthalic acid and ethylene glycol in a molar ratio of 1:1.4 are used as polyester monomers. Based on the mass of the polyester monomer, 250 ppm of catalyst ethylene glycol antimony and 2 wt % of diatomaceous earth with a particle size of 500 nm are added to the polyester monomer; under a nitrogen atmosphere, esterification is first performed at 210° C. at normal pressure for 30 min, and then at 240° C. and 0.3 MPa under pressure for 120 min to obtain an esterified product.

[0031] (2) polycondensation reaction: adding 5-(sodium sulfonated)isotitanic acid and polyethylene glycol with a molecular weight of 1000 g / mol to the esterified product, wherein the molar ratio of 5-(sodium sulfonated)isotitanic acid to terephthalic acid in step (1) is 1:100, and the amount of polyethylene glycol added is 1 wt% of the mass of the polyester monomer in step (1); performing negative compression polymerization at 275° C. under vacuum conditions for 1.5 h, and then stopping the reaction to obtain modified polyester, and preparing modified polyester chips by conventional methods.

[0032] (3) Spinning: The modified polyester chips were vacuum dried at 100°C for 24 hours, and then added to a screw spinning machine for melt metering and spun through a hollow cross-section spinneret, wherein the spinning temperature was 280°C and the spinning winding speed was 3000 m / min, to obtain a hollow structured modified polyester fiber.

[0033] (4) Pore formation: The polyester fiber is alkaline washed in a sodium hydroxide aqueous solution at 80°C and a concentration of 1.5 mol / L for 30 min to react with the diatomaceous earth exposed on the surface of the hollow fiber to form pores, and the polyester matrix is ​​further etched to form a porous structure on the fiber surface. The fiber is then washed with water and dried to finally obtain a moisture-absorbing and perspiration-wicking polyester fiber.

[0034] Example 3 The difference from Example 1 is that the amount of hydrophilic monomer used in step (2) is increased.

[0035] A method for preparing a moisture absorbing and perspiration wicking polyester fiber, comprising the following steps: (1) Esterification reaction: terephthalic acid and ethylene glycol in a molar ratio of 1:1.4 are used as polyester monomers. Based on the mass of the polyester monomer, 250 ppm of catalyst ethylene glycol antimony and 2 wt % of diatomaceous earth with a particle size of 500 nm are added to the polyester monomer; under a nitrogen atmosphere, esterification is first performed at 210° C. at normal pressure for 30 min, and then at 240° C. and 0.3 MPa under pressure for 120 min to obtain an esterified product.

[0036] (2) polycondensation reaction: adding 5-(sodium sulfonated)isotitanic acid and polyethylene glycol with a molecular weight of 4000 g / mol to the esterified product, wherein the molar ratio of 5-(sodium sulfonated)isotitanic acid to terephthalic acid in step (1) is 1:20, and the amount of polyethylene glycol added is 5 wt% of the mass of the polyester monomer in step (1); performing negative compression polymerization at 280° C. for 1 h under vacuum conditions, and then stopping the reaction to obtain modified polyester, and preparing modified polyester chips by conventional methods.

[0037] (3) Spinning: The modified polyester chips were vacuum dried at 100°C for 24 hours, and then added to a screw spinning machine for melt metering and spun through a hollow cross-section spinneret, wherein the spinning temperature was 280°C and the spinning winding speed was 3000 m / min, to obtain a hollow structured modified polyester fiber.

[0038] (4) Pore formation: The polyester fiber is alkaline washed in a sodium hydroxide aqueous solution at 80°C and a concentration of 1.5 mol / L for 30 min to react with the diatomaceous earth exposed on the surface of the hollow fiber to form pores, and the polyester matrix is ​​further etched to form a porous structure on the fiber surface. The fiber is then washed with water and dried to finally obtain a moisture-absorbing and perspiration-wicking polyester fiber.

[0039] Example 4 The difference from Example 1 is that the diatomaceous earth particle size in step (1) is smaller.

[0040] A method for preparing a moisture absorbing and perspiration wicking polyester fiber, comprising the following steps: (1) Esterification reaction: terephthalic acid and ethylene glycol in a molar ratio of 1:1.4 are used as polyester monomers. Based on the mass of the polyester monomer, 250 ppm of catalyst ethylene glycol antimony and 2 wt % of diatomaceous earth with a particle size of 200 nm are added to the polyester monomer; under a nitrogen atmosphere, esterification is first performed at 210° C. at normal pressure for 30 minutes, and then at 240° C. and 0.3 MPa under pressure for 120 minutes to obtain an esterified product.

[0041] (2) polycondensation reaction: adding 5-(sodium sulfonated)isotitanic acid and polyethylene glycol with a molecular weight of 2000 g / mol to the esterified product, wherein the molar ratio of 5-(sodium sulfonated)isotitanic acid to terephthalic acid in step (1) is 1:50, and the amount of polyethylene glycol added is 2 wt% of the mass of the polyester monomer in step (1); performing negative compression polymerization at 278° C. for 1 h under vacuum conditions, and then stopping the reaction to obtain modified polyester, and preparing modified polyester chips by conventional methods.

[0042] (3) Spinning: The modified polyester chips were vacuum dried at 100°C for 24 hours, and then added to a screw spinning machine for melt metering and spun through a hollow cross-section spinneret, wherein the spinning temperature was 280°C and the spinning winding speed was 3000 m / min, to obtain a hollow structured modified polyester fiber.

[0043] (4) Pore formation: The polyester fiber is alkaline washed in a sodium hydroxide aqueous solution at 80°C and a concentration of 1.5 mol / L for 30 min to react with the diatomaceous earth exposed on the surface of the hollow fiber to form pores, and the polyester matrix is ​​further etched to form a porous structure on the fiber surface. The fiber is then washed with water and dried to finally obtain a moisture-absorbing and perspiration-wicking polyester fiber.

[0044] Example 5 The difference from Example 1 is that the diatomaceous earth particles in step (1) are larger in size.

[0045] A method for preparing a moisture absorbing and perspiration wicking polyester fiber, comprising the following steps: (1) Esterification reaction: terephthalic acid and ethylene glycol in a molar ratio of 1:1.4 are used as polyester monomers. Based on the mass of the polyester monomer, 250 ppm of catalyst ethylene glycol antimony and 2 wt % of diatomaceous earth with a particle size of 800 nm are added to the polyester monomer; under a nitrogen atmosphere, esterification is first performed at 210° C. at normal pressure for 30 min, and then at 240° C. and 0.3 MPa under pressure for 120 min to obtain an esterified product.

[0046] (2) polycondensation reaction: adding 5-(sodium sulfonated)isotitanic acid and polyethylene glycol with a molecular weight of 2000 g / mol to the esterified product, wherein the molar ratio of 5-(sodium sulfonated)isotitanic acid to terephthalic acid in step (1) is 1:50, and the amount of polyethylene glycol added is 2 wt% of the mass of the polyester monomer in step (1); performing negative compression polymerization at 278° C. for 1 h under vacuum conditions, and then stopping the reaction to obtain modified polyester, and preparing modified polyester chips by conventional methods.

[0047] (3) Spinning: The modified polyester chips were vacuum dried at 100°C for 24 hours, and then added to a screw spinning machine for melt metering and spun through a hollow cross-section spinneret, wherein the spinning temperature was 280°C and the spinning winding speed was 3000 m / min, to obtain a hollow structured modified polyester fiber.

[0048] (4) Pore formation: The polyester fiber is alkaline washed in a sodium hydroxide aqueous solution at 80°C and a concentration of 1.5 mol / L for 30 min to react with the diatomaceous earth exposed on the surface of the hollow fiber to form pores, and the polyester matrix is ​​further etched to form a porous structure on the fiber surface. The fiber is then washed with water and dried to finally obtain a moisture-absorbing and perspiration-wicking polyester fiber.

[0049] Example 6 The difference from Example 1 is that the content of diatomaceous earth in step (1) is less.

[0050] A method for preparing a moisture absorbing and perspiration wicking polyester fiber, comprising the following steps: (1) Esterification reaction: terephthalic acid and ethylene glycol in a molar ratio of 1:1.1 are used as polyester monomers. Based on the mass of the polyester monomer, 100 ppm of catalyst titanium glycolate and 0.1 wt % of diatomaceous earth with a particle size of 500 nm are added to the polyester monomer; under a nitrogen atmosphere, esterification is first carried out at 200° C. and normal pressure for 50 min, and then at 220° C. and 0.2 MPa for 180 min to obtain an esterified product.

[0051] (2) polycondensation reaction: adding 5-(sodium sulfonated)isotitanic acid and polyethylene glycol with a molecular weight of 600 g / mol to the esterified product, wherein the molar ratio of 5-(sodium sulfonated)isotitanic acid to terephthalic acid in step (1) is 1:20, and the amount of polyethylene glycol added is 5 wt% of the mass of the polyester monomer in step (1); performing negative compression polymerization at 260° C. for 2 h under vacuum conditions, and then stopping the reaction to obtain modified polyester, and preparing modified polyester chips by conventional methods.

[0052] (3) Spinning: The modified polyester chips were vacuum dried at 60°C for 30 hours, and then added to a screw spinning machine for melt metering and spun through a hollow cross-section spinneret, wherein the spinning temperature was 260°C and the spinning winding speed was 4000 m / min, to obtain a hollow structured modified polyester fiber.

[0053] (4) Pore formation: The polyester fiber is alkaline washed in a sodium hydroxide aqueous solution at 80°C and a concentration of 1.5 mol / L for 30 min to react with the diatomaceous earth exposed on the surface of the hollow fiber to form pores, and the polyester matrix is ​​further etched to form a porous structure on the fiber surface. The fiber is then washed with water and dried to finally obtain a moisture-absorbing and perspiration-wicking polyester fiber.

[0054] Example 7 The difference from Example 1 is that the content of diatomaceous earth in step (1) is relatively high.

[0055] A method for preparing a moisture absorbing and perspiration wicking polyester fiber, comprising the following steps: (1) Esterification reaction: terephthalic acid and ethylene glycol in a molar ratio of 1:1.1 are used as polyester monomers. Based on the mass of the polyester monomer, 100 ppm of catalyst titanium glycol and 5 wt% of diatomaceous earth with a particle size of 500 nm are added to the polyester monomer; under a nitrogen atmosphere, esterification is first carried out at 200° C. and normal pressure for 50 min, and then at 220° C. and 0.2 MPa for 180 min to obtain an esterified product.

[0056] (2) polycondensation reaction: adding 5-(sodium sulfonated)isotitanic acid and polyethylene glycol with a molecular weight of 600 g / mol to the esterified product, wherein the molar ratio of 5-(sodium sulfonated)isotitanic acid to terephthalic acid in step (1) is 1:20, and the amount of polyethylene glycol added is 5 wt% of the mass of the polyester monomer in step (1); performing negative compression polymerization at 260° C. for 2 h under vacuum conditions, and then stopping the reaction to obtain modified polyester, and preparing modified polyester chips by conventional methods.

[0057] (3) Spinning: The modified polyester chips were vacuum dried at 60°C for 30 hours, and then added to a screw spinning machine for melt metering and spun through a hollow cross-section spinneret, wherein the spinning temperature was 260°C and the spinning winding speed was 4000 m / min, to obtain a hollow structured modified polyester fiber.

[0058] (4) Pore formation: The polyester fiber is alkaline washed in a sodium hydroxide aqueous solution at 80°C and a concentration of 1.5 mol / L for 30 min to react with the diatomaceous earth exposed on the surface of the hollow fiber to form pores, and the polyester matrix is ​​further etched to form a porous structure on the fiber surface. The fiber is then washed with water and dried to finally obtain a moisture-absorbing and perspiration-wicking polyester fiber.

[0059] Example 8 The difference from Example 1 is that the alkali treatment in step (3) is milder.

[0060] A method for preparing a moisture absorbing and perspiration wicking polyester fiber, comprising the following steps: (1) Esterification reaction: terephthalic acid and ethylene glycol in a molar ratio of 1:1.4 are used as polyester monomers. Based on the mass of the polyester monomer, 250 ppm of catalyst ethylene glycol antimony and 2 wt % of diatomaceous earth with a particle size of 500 nm are added to the polyester monomer; under a nitrogen atmosphere, esterification is first performed at 210° C. at normal pressure for 30 min, and then at 240° C. and 0.3 MPa under pressure for 120 min to obtain an esterified product.

[0061] (2) polycondensation reaction: adding 5-(sodium sulfonated)isotitanic acid and polyethylene glycol with a molecular weight of 2000 g / mol to the esterified product, wherein the molar ratio of 5-(sodium sulfonated)isotitanic acid to terephthalic acid in step (1) is 1:50, and the amount of polyethylene glycol added is 2 wt% of the mass of the polyester monomer in step (1); performing negative compression polymerization at 278° C. for 1 h under vacuum conditions, and then stopping the reaction to obtain modified polyester, and preparing modified polyester chips by conventional methods.

[0062] (3) Spinning: The modified polyester chips were vacuum dried at 100°C for 24 hours, and then added to a screw spinning machine for melt metering and spun through a hollow cross-section spinneret, wherein the spinning temperature was 280°C and the spinning winding speed was 3000 m / min, to obtain a hollow structured modified polyester fiber.

[0063] (4) Pore formation: The polyester fiber is alkaline washed in a 1.5 mol / L sodium hydroxide aqueous solution at 60°C for 30 min to react with the diatomaceous earth exposed on the surface of the hollow fiber to form pores, and the polyester matrix is ​​further etched to form a porous structure on the fiber surface. The fiber is then washed and dried to finally obtain a moisture-absorbing and perspiration-wicking polyester fiber.

[0064] Example 9 The difference from Example 1 is that the alkali treatment is more severe.

[0065] A method for preparing a moisture absorbing and perspiration wicking polyester fiber, comprising the following steps: (1) Esterification reaction: terephthalic acid and ethylene glycol in a molar ratio of 1:1.4 are used as polyester monomers. Based on the mass of the polyester monomer, 250 ppm of catalyst ethylene glycol antimony and 2 wt % of diatomaceous earth with a particle size of 500 nm are added to the polyester monomer; under a nitrogen atmosphere, esterification is first performed at 210° C. at normal pressure for 30 min, and then at 240° C. and 0.3 MPa under pressure for 120 min to obtain an esterified product.

[0066] (2) polycondensation reaction: adding 5-(sodium sulfonated)isotitanic acid and polyethylene glycol with a molecular weight of 2000 g / mol to the esterified product, wherein the molar ratio of 5-(sodium sulfonated)isotitanic acid to terephthalic acid in step (1) is 1:50, and the amount of polyethylene glycol added is 2 wt% of the mass of the polyester monomer in step (1); performing negative compression polymerization at 278° C. for 1 h under vacuum conditions, and then stopping the reaction to obtain modified polyester, and preparing modified polyester chips by conventional methods.

[0067] (3) Spinning: The modified polyester chips were vacuum dried at 100°C for 24 hours, and then added to a screw spinning machine for melt metering and spun through a hollow cross-section spinneret, wherein the spinning temperature was 280°C and the spinning winding speed was 3000 m / min, to obtain a hollow structured modified polyester fiber.

[0068] (4) Pore formation: The polyester fiber is alkaline washed in sodium hydroxide at 90°C and a concentration of 2.0 mol / L for 50 min to react with the diatomaceous earth exposed on the surface of the hollow fiber to form pores, and the polyester matrix is ​​further etched to form a porous structure on the fiber surface. The fiber is then washed with water and dried to finally obtain a moisture-absorbing and perspiration-wicking polyester fiber.

[0069] Comparative Example 1 The difference from Example 1 is that no 5-(sodium sulfonate)isotitanic acid is added during the polycondensation in step (2).

[0070] A method for preparing polyester fiber, comprising the following steps: (1) Esterification reaction: terephthalic acid and ethylene glycol in a molar ratio of 1:1.4 are used as polyester monomers. Based on the mass of the polyester monomer, 250 ppm of catalyst ethylene glycol antimony and 2 wt % of diatomaceous earth with a particle size of 500 nm are added to the polyester monomer; under a nitrogen atmosphere, esterification is first performed at 210° C. at normal pressure for 30 min, and then at 240° C. and 0.3 MPa under pressure for 120 min to obtain an esterified product.

[0071] (2) polycondensation reaction: adding polyethylene glycol with a molecular weight of 2000 g / mol to the esterified product, wherein the amount of polyethylene glycol added is 1 wt% of the mass of the polyester monomer in step (1); performing negative compression polymerization at 278° C. under vacuum conditions for 1 h, and then stopping the reaction to obtain modified polyester, and preparing modified polyester chips by conventional methods.

[0072] (3) Spinning: The modified polyester chips were vacuum dried at 100°C for 24 hours, and then added to a screw spinning machine for melt metering and spun through a hollow cross-section spinneret, wherein the spinning temperature was 280°C and the spinning winding speed was 3000 m / min, to obtain a hollow structured modified polyester fiber.

[0073] (4) Pore formation: The polyester fiber is alkaline washed in sodium hydroxide at 80°C and a concentration of 1.5 mol / L for 30 min to react with the diatomaceous earth exposed on the surface of the hollow fiber to form pores, and the polyester matrix is ​​further etched to form a porous structure on the fiber surface. The fiber is then washed with water and dried to finally obtain a moisture-absorbing and perspiration-wicking polyester fiber.

[0074] Comparative Example 2 The difference from Example 1 is that polyethylene glycol is not added in step (2).

[0075] A method for preparing polyester fiber, comprising the following steps: (1) Esterification reaction: terephthalic acid and ethylene glycol in a molar ratio of 1:1.4 are used as polyester monomers. Based on the mass of the polyester monomer, 250 ppm of catalyst ethylene glycol antimony and 2 wt % of diatomaceous earth with a particle size of 500 nm are added to the polyester monomer; under a nitrogen atmosphere, esterification is first performed at 210° C. at normal pressure for 30 min, and then at 240° C. and 0.3 MPa under pressure for 120 min to obtain an esterified product.

[0076] (2) polycondensation reaction: adding 5-(sodium sulfonated)isotitanic acid to the esterified product, wherein the molar ratio of 5-(sodium sulfonated)isotitanic acid to the terephthalic acid in step (1) is 1:50; performing negative compression polymerization at 278° C. under vacuum conditions for 1 h, and then stopping the reaction to obtain a modified polyester, and preparing the modified polyester chips by a conventional method.

[0077] (3) Spinning: The modified polyester chips were vacuum dried at 100°C for 24 hours, and then added to a screw spinning machine for melt metering and spun through a hollow cross-section spinneret, wherein the spinning temperature was 280°C and the spinning winding speed was 3000 m / min, to obtain a hollow structured modified polyester fiber.

[0078] (4) Pore formation: The polyester fiber is alkaline washed in a sodium hydroxide aqueous solution at 80°C and a concentration of 1.5 mol / L for 30 min to react with the diatomaceous earth exposed on the surface of the hollow fiber to form pores, and the polyester matrix is ​​further etched to form a porous structure on the fiber surface. The fiber is then washed with water and dried to finally obtain a moisture-absorbing and perspiration-wicking polyester fiber.

[0079] Comparative Example 3 The difference from Example 1 is that diatomaceous earth is not added during the esterification in step (1).

[0080] A method for preparing polyester fiber, comprising the following steps: (1) Esterification reaction: terephthalic acid and ethylene glycol in a molar ratio of 1:1.4 are used as polyester monomers, and 250 ppm of catalyst ethylene glycol antimony is added to the polyester monomer based on the mass of the polyester monomer; under a nitrogen atmosphere, esterification is first carried out at 210° C. and normal pressure for 30 minutes, and then at 240° C. and 0.3 MPa for 120 minutes under pressure to obtain an esterified product.

[0081] (2) polycondensation reaction: adding 5-(sodium sulfonated)isotitanic acid and polyethylene glycol with a molecular weight of 2000 g / mol to the esterified product, wherein the molar ratio of 5-(sodium sulfonated)isotitanic acid to terephthalic acid in step (1) is 1:50, and the amount of polyethylene glycol added is 2 wt% of the mass of the polyester monomer in step (1); performing negative compression polymerization at 278° C. for 1 h under vacuum conditions, and then stopping the reaction to obtain modified polyester, and preparing modified polyester chips by conventional methods.

[0082] (3) Spinning: The modified polyester chips were vacuum dried at 100°C for 24 hours, and then added to a screw spinning machine for melt metering and spun through a hollow cross-section spinneret, wherein the spinning temperature was 280°C and the spinning winding speed was 3000 m / min, to obtain a hollow structured modified polyester fiber.

[0083] (4) Alkaline bath: The polyester fiber is alkaline washed in 1.5 mol / L sodium hydroxide at 80°C for 30 min to etch the polyester matrix, and then washed with water and dried to finally obtain a moisture wicking polyester fiber.

[0084] Comparative Example 4 The difference from Example 1 is that step (3) does not use a hollow cross-section spinneret.

[0085] A method for preparing polyester fiber, comprising the following steps: (1) Esterification reaction: terephthalic acid and ethylene glycol in a molar ratio of 1:1.4 are used as polyester monomers. Based on the mass of the polyester monomer, 250 ppm of catalyst ethylene glycol antimony and 2 wt % of diatomaceous earth with a particle size of 500 nm are added to the polyester monomer; under a nitrogen atmosphere, esterification is first performed at 210° C. at normal pressure for 30 min, and then at 240° C. and 0.3 MPa under pressure for 120 min to obtain an esterified product.

[0086] (2) polycondensation reaction: adding 5-(sodium sulfonated)isotitanic acid and polyethylene glycol with a molecular weight of 2000 g / mol to the esterified product, wherein the molar ratio of 5-(sodium sulfonated)isotitanic acid to terephthalic acid in step (1) is 1:50, and the amount of polyethylene glycol added is 2 wt% of the mass of the polyester monomer in step (1); performing negative compression polymerization at 278° C. for 1 h under vacuum conditions, and then stopping the reaction to obtain modified polyester, and preparing modified polyester chips by conventional methods.

[0087] (3) Spinning: The modified polyester chips were vacuum dried at 100°C for 24 hours, and then added to a screw spinning machine for melt metering and spun through a conventional circular cross-section spinneret, wherein the spinning temperature was 280°C and the spinning winding speed was 3000 m / min, to obtain a hollow structured modified polyester fiber.

[0088] (4) Pore preparation: The polyester fiber is alkaline washed in 1.5 mol / L sodium hydroxide at 80°C for 30 min, reacted with diatomaceous earth to form pores, and the polyester matrix is ​​further etched to form a porous structure on the fiber surface. The fiber is then washed and dried to obtain a moisture-absorbing and perspiration-wicking polyester fiber.

[0089] Comparative Example 5 The difference from Example 1 is that the particle size of diatomaceous earth exceeds the preferred range.

[0090] A method for preparing polyester fiber, comprising the following steps: (1) Esterification reaction: terephthalic acid and ethylene glycol in a molar ratio of 1:1.4 are used as polyester monomers. Based on the mass of the polyester monomer, 250 ppm of catalyst ethylene glycol antimony and 2 wt % of diatomaceous earth with a particle size of 1200 nm are added to the polyester monomer; under a nitrogen atmosphere, esterification is first performed at 210° C. at normal pressure for 30 min, and then at 240° C. and 0.3 MPa under pressure for 120 min to obtain an esterified product.

[0091] (2) polycondensation reaction: adding 5-(sodium sulfonated)isotitanic acid and polyethylene glycol with a molecular weight of 2000 g / mol to the esterified product, wherein the molar ratio of 5-(sodium sulfonated)isotitanic acid to terephthalic acid in step (1) is 1:50, and the amount of polyethylene glycol added is 1 wt% of the mass of the polyester monomer in step (1); performing negative compression polymerization at 278° C. for 1 h under vacuum conditions, and then stopping the reaction to obtain modified polyester, and preparing modified polyester chips by conventional methods.

[0092] (3) Spinning: The modified polyester chips were vacuum dried at 100°C for 24 hours, and then added to a screw spinning machine for melt metering and spun through a hollow cross-section spinneret, wherein the spinning temperature was 280°C and the spinning winding speed was 3000 m / min, to obtain a hollow structured modified polyester fiber.

[0093] (4) Pore formation: The polyester fiber is alkaline washed in a sodium hydroxide aqueous solution at 80°C and a concentration of 1.5 mol / L for 30 min to react with the diatomaceous earth exposed on the surface of the hollow fiber to form pores, and the polyester matrix is ​​further etched to form a porous structure on the fiber surface. The fiber is then washed with water and dried to finally obtain a moisture-absorbing and perspiration-wicking polyester fiber.

[0094] Comparative Example 6 The difference from Example 1 is that the diatomaceous earth in step (1) is replaced by pure amorphous silicon dioxide.

[0095] A method for preparing polyester fiber, comprising the following steps: (1) Esterification reaction: terephthalic acid and ethylene glycol in a molar ratio of 1:1.4 are used as polyester monomers. Based on the mass of the polyester monomer, 250 ppm of catalyst ethylene glycol antimony and 2 wt % of amorphous silica with a particle size of 500 nm are added to the polyester monomer; under a nitrogen atmosphere, esterification is first performed at 210° C. at normal pressure for 30 min, and then at 240° C. and 0.3 MPa under pressure for 120 min to obtain an esterified product.

[0096] (2) polycondensation reaction: adding 5-(sodium sulfonated)isotitanic acid and polyethylene glycol with a molecular weight of 2000 g / mol to the esterified product, wherein the molar ratio of 5-(sodium sulfonated)isotitanic acid to terephthalic acid in step (1) is 1:50, and the amount of polyethylene glycol added is 2 wt% of the mass of the polyester monomer in step (1); performing negative compression polymerization at 278° C. for 1 h under vacuum conditions, and then stopping the reaction to obtain modified polyester, and preparing modified polyester chips by conventional methods.

[0097] (3) Spinning: The modified polyester chips were vacuum dried at 100°C for 24 hours, and then added to a screw spinning machine for melt metering and spun through a hollow cross-section spinneret, wherein the spinning temperature was 280°C and the spinning winding speed was 3000 m / min, to obtain a hollow structured modified polyester fiber.

[0098] (4) Pore formation: The polyester fiber is alkaline washed in a 1.5 mol / L sodium hydroxide aqueous solution at 80°C for 30 min to react with the amorphous silica exposed on the surface of the hollow fiber to form pores, and the polyester matrix is ​​further etched to form a porous structure on the fiber surface. The fiber is then washed and dried to obtain a moisture-absorbing and perspiration-wicking polyester fiber.

[0099] Performance Testing The performance of the moisture wicking polyester fiber prepared in each embodiment and comparative example was tested, and the testing method was as follows: (1) the tensile strength and elongation at break of the moisture wicking polyester fiber were evaluated according to the standard GB / T 14344-2022 "Test method for tensile properties of chemical fiber filaments"; (2) the moisture wicking polyester fiber was evaluated for its moisture absorption and quick-drying performance after knitting, referring to GB / T21655.1-2008 "Evaluation of moisture absorption and quick-drying properties of textiles", the moisture absorption performance was mainly evaluated by the wicking height, and the quick-drying performance was mainly evaluated by the evaporation rate.

[0100] The test results are shown in Table 1.

[0101] Table 1. Performance indicators of moisture wicking polyester fibers and fabrics Tensile strength (cN / dtex) Elongation at break (%) Wicking height (mm) Evaporation rate (g / h) Example 1 3.2 28 141 0.51 Example 2 3.3 30 135 0.53 Example 3 2.9 27 146 0.48 Example 4 3.3 29 145 0.54 Example 5 2.7 27 138 0.47 Example 6 3.4 29 136 0.46 Example 7 2.9 26 146 0.55 Example 8 3.3 27 128 0.45 Example 9 2.8 24 145 0.54 Comparative Example 1 3.5 30 105 0.53 Comparative Example 2 3.4 28 108 0.53 Comparative Example 3 3.6 26 116 0.38 Comparative Example 4 4.0 29 98 0.32 Comparative Example 5 2.4 24 128 0.38 Comparative Example 6 2.9 25 137 0.47 From Table 1 we can see that: (1) The present invention introduces hydrophilic groups, spins hollow structure fibers, and nano-diatomaceous earth that can react with alkali and a polyester matrix to prepare polyester fibers with moisture absorption and perspiration removal properties. By comparing the performance test results of Example 1 and Comparative Examples 1-4, it can be found that the introduction of hydrophilic groups, the cross-section of the hollow structure, and the alkali dissolution treatment all have a positive effect on the improvement of the moisture absorption and perspiration removal properties of the polyester fibers. The combination of the three has the best modification effect, but it is also necessary to pay attention to its mechanical properties at the same time so that it meets the use requirements.

[0102] (2) By comparing the performance test results of Examples 1-3, it can be found that as the content of hydrophilic groups increases, the hygroscopicity of the polyester fiber increases, but the mechanical properties and quick-drying properties decrease.

[0103] (3) By comparing the performance test results of Example 1 with Examples 4-7 and Comparative Example 5, it can be found that reducing the particle size of nano-diatomaceous earth and increasing its content can effectively improve the moisture absorption and perspiration management of polyester fiber, but too much content or too large a particle size will cause a loss of its mechanical properties.

[0104] (4) By comparing the performance test results of Example 1 with those of Examples 8 and 9, it can be found that more stringent alkali dissolution treatment conditions can form more fiber structural defects, thereby improving its moisture absorption and perspiration performance, but its mechanical properties also deteriorate more seriously.

[0105] (5) Comparing the performance test results of Example 1 and Comparative Example 6, the effect of using pure silicon dioxide is not as good as diatomaceous earth. The main component of diatomaceous earth is amorphous silicon dioxide, which easily reacts with chemical reagents to form pores. Diatomaceous earth also contains a small amount of Al2O3, Fe2O3, CaO, MgO, K2O, Na2O, P2O5 and organic matter. After reacting with chemical reagents, it will leave a skeleton to improve the mechanical properties of the fiber. The trace elements therein also have a certain promoting effect on moisture absorption and perspiration, while pure silicon dioxide does not have these effects.

[0106] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.

Claims

1. A method for preparing a moisture wicking polyester fiber, characterized in that: The following steps are involved: (1) Esterification reaction: Add nano-diatomaceous earth to polyester monomer to carry out esterification reaction to obtain esterified product; (2) Polycondensation reaction: Add 5-(sodium sulfo)isotitanic acid and polyethylene glycol to the esterified product to carry out polycondensation reaction to obtain modified polyester chips; (3) Spinning: The modified polyester chips are melt-spinned to produce hollow polyester fibers; (4) Hole making: chemical reagents are mixed with hollow polyester fibers, and the chemical reagents react to remove at least a portion of the nano-diatomaceous earth, so that holes are formed in the hollow fibers. After washing and drying, moisture-absorbing and sweat-wicking polyester fibers are obtained.

2. The method for preparing a moisture wicking polyester fiber according to claim 1, characterized in that: The particle size of the nano-diatomite is 200-800 nm; the addition amount of the nano-diatomite is 0.1-5wt% of the polyester monomer.

3. The method for preparing a moisture wicking polyester fiber according to claim 1 or 2, characterized in that: The polyester monomers are terephthalic acid and ethylene glycol in a molar ratio of 1:1.1~1.

5.

4. The method for preparing a moisture wicking polyester fiber according to claim 1, characterized in that: The catalyst for the esterification reaction is one of ethylene glycol antimony, ethylene glycol titanium or tetrabutyl titanate, and the added amount is 100-400 ppm of the polyester monomer.

5. The method for preparing a moisture wicking polyester fiber according to claim 1 or 4, characterized in that: The conditions of the esterification reaction are: under an inert atmosphere, first esterify at 200~220 ºC under normal pressure for 20~50 min, and then esterify under pressure at 220~250 ºC and 0.2~0.4 MPa for 80~180 min.

6. The method for preparing a moisture wicking polyester fiber according to claim 1, characterized in that: The molar ratio of 5-(sodium sulfonate)isotitanic acid to terephthalic acid is 1:20-100.

7. The method for preparing a moisture wicking polyester fiber according to claim 1, characterized in that: The molecular weight of the polyethylene glycol in step (2) is 600-4000 g / mol, and the amount added is 1-5 wt% of the polyester monomer.

8. The method for preparing a moisture wicking polyester fiber according to claim 1, 6 or 7, characterized in that: The conditions of the polycondensation reaction are: negative compression polymerization at 260~280 ºC for 0.5~2 h under vacuum conditions.

9. The method for preparing a moisture wicking polyester fiber according to claim 1, characterized in that: The spinning process is as follows: the modified polyester chips are vacuum dried at 60-120 ºC for 10-30 hours, then added to a screw spinning machine for melt metering and spun through a hollow cross-section spinneret, wherein the spinning temperature is 260-290 ºC and the spinning winding speed is 2500-4000 m / min.

10. The method for preparing a moisture wicking polyester fiber according to claim 1 or 9, characterized in that: The chemical reagent is alkali solution, and the washing process is: wash the vacuum polyester fiber in alkali solution with a temperature of 60-90 ºC and a concentration of 1.5-2.0 mol / L for 30-50 min.

Citation Information

Patent Citations

  • Moisture absorption and sweat discharge fiber

    CN104372428A

  • Moisture absorbing and sweat releasing polyvinyl chloride fiber

    CN105543996A

  • Multi-micropore polyester fiber and preparation method thereof

    CN101144206A

  • Method for producing modified cation polyester filament and product thereof

    CN102094256A

  • A hygroscopic polyester fiber and its production method

    CN102296377A

Cited By

  • Moisture absorption and sweat releasing profiled fiber

    CN116103783A

  • High-moisture-absorption low-fuzzing and pilling regenerated polyester fiber and blended yarn prepared from same

    CN122257145A

  • High moisture-absorbing and low fuzzing and pilling regenerated polyester fiber and preparation of blended yarn thereof

    CN122257145B