Antibacterial and crease-resistant fabric and preparation process
Through ultrasonic treatment and impregnation processes, nano zinc oxide, chitosan and graphene oxide and other materials were combined to prepare fabric fabrics with significant antibacterial and wrinkle resistance, which solved the problem of insufficient antibacterial and wrinkle resistance of existing fabric fabrics. Improves the market value and application prospects of the product.
Patent Information
- Application Number
- CN202411274335.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing fabrics have shortcomings in antibacterial properties and wrinkle resistance, and the comfort and wrinkle resistance of textiles need to be further improved, which affects the grade and market value of the product.
Using ultrasonic treatment and impregnation process, nano zinc oxide, chitosan and crosslinking agent are mixed and combined with graphene oxide, coupling agent and glycerin. Antibacterial and wrinkle fabrics are prepared through stirring and dipping steps to improve the antibacterial properties of the fabrics. and wrinkle resistance.
It significantly enhances the antibacterial and wrinkle resistance of the fabric, making it more suitable for market demand, suitable for industrial production, and improves the overall performance of the fabric.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fabrics and relates to an antibacterial and wrinkle-resistant fabric and a preparation process. Background Art
[0002] Fabrics provide a good living space for pathogenic fungi due to their porous structure and good moisture absorption. Studies have shown that patients may directly or indirectly transmit pathogenic fungi to other normal people through skin contact or skin scales. Therefore, textiles touched by people with superficial fungal diseases can be transmitted to others as pathogen carriers. At the same time, with the development of people's aesthetics, the beauty of fabrics is also an important factor affecting their value. Many cotton, knitted and other fabrics are prone to wrinkling and not draping. Regenerated cellulose products are increasingly favored by consumers. However, textiles of these fiber varieties have the disadvantages of poor elasticity and easy wrinkling, and poor appearance shape retention, which reduces the grade of the product.
[0003] The antibacterial finishing agent in the prior art is not very dispersible on the textile fabric, which affects the antibacterial performance of the textile fabric, and the comfort and wrinkle resistance of the fabric need to be further improved.
[0004] Therefore, optimizing the comprehensive performance of the fabric to make the anti-wrinkle and antibacterial effects more significant, and the anti-wrinkle and antibacterial fabrics with higher added value meet the market demand; and optimizing its process flow and simplifying the production raw materials to achieve the same antibacterial and anti-wrinkle performance have broad market value and application prospects, and are of great significance to promoting the development of the functional fabric industry. Summary of the invention
[0005] The purpose of the present invention is to provide an antibacterial and wrinkle-resistant fabric and a preparation process thereof.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A preparation process of an antibacterial and wrinkle-resistant fabric comprises the following steps:
[0008] M1: Add the fabric into an alkali solution with a mass fraction of 5 to 10% for ultrasonic treatment and soak for 1 to 1.5 hours before taking it out. Then, the fabric is ultrasonically washed with deionized water and dried to obtain the pretreated fabric for use.
[0009] M2: Mix nano zinc oxide, chitosan and cross-linking agent at room temperature to obtain mixed solution A, then add the pretreated fabric into the mixed solution A and stir, heat to 60-70°C and continue stirring for 4-6 hours. After the reaction, ultrasonically wash with deionized water and dry to constant weight.
[0010] M3: Add graphene oxide, coupling agent and glycerol into deionized water and mix and stir to obtain a mixed solution B, then place the fabric treated with M2 in the mixed solution B for immersion, and ultrasonically wash the fabric with deionized water, and finally dry it to constant weight to obtain the antibacterial and wrinkle-resistant fabric of the present invention.
[0011] As a preferred technical solution of the present invention, the ultrasonic frequency is 45 to 70 Hz, and the ultrasonic time is 20 to 30 minutes.
[0012] As a preferred technical solution of the present invention, the crosslinking agent in M2 is made of vinyltrimethylsilane and aminoformylhydrazide in a molar ratio of 1:5, and the preparation method is as follows:
[0013] Weigh a certain amount of aminoformyl hydrazide and water and add them into a reaction container, control the reaction container to be cooled to a constant temperature in an ice water bath, then add vinyltrimethylsilane dropwise into the reaction container, stir and react in an ice water bath for 30 to 40 minutes after the addition is complete, then heat to room temperature and stir and react for 2 to 3 hours, then perform reduced pressure distillation to obtain a cross-linking agent.
[0014] As a preferred technical solution of the present invention, the stirring speed in M2 is 220 to 300 rpm, and the stirring time before heating is 10 to 20 min.
[0015] As a preferred technical solution of the present invention, the particle size of the nano zinc oxide is 10 to 20 μm.
[0016] As a preferred technical solution of the present invention, the mass ratio of the nano zinc oxide, chitosan and cross-linking agent is 3:4:5-7.5.
[0017] As a preferred technical solution of the present invention, the padding time in M3 is 2 to 4 hours, and the drying temperature is 45 to 60°C.
[0018] As a preferred technical solution of the present invention, the mass ratio of the graphene oxide, the coupling agent, the glycerol and the deionized water is 2-3:3-5:1.5:3, and the coupling agent is any one of KH602, KH580 and KH550.
[0019] An antibacterial and wrinkle-resistant fabric is prepared by the above-mentioned preparation process.
[0020] As a preferred technical solution of the present invention, the fabric is a knitted fabric.
[0021] Beneficial effects of the present invention:
[0022] (1) In the preparation process of the antibacterial and wrinkle-proof fabric of the present invention, vinyl trimethylsilane and aminoformyl hydrazide are used to prepare a crosslinking agent, and the crosslinking agent is used together with nano zinc oxide and chitosan to prepare the antibacterial fabric. The amino group on aminoformyl hydrazide can graft the nano zinc oxide and chitosan onto the fabric after pretreatment, and the antibacterial property of the fabric after adsorbing the nano zinc oxide and chitosan is significantly enhanced; at the same time, vinyl trimethylsilane reacts with aminoformyl hydrazide, that is, the double bond on the vinyl trimethylsilane is broken, replacing the hydrogen atoms on the amino group on the aminoformyl hydrazide, and the abundant methyl group of the vinyl trimethylsilane can increase the steric hindrance between the substances, so that the nano zinc oxide and chitosan are more evenly distributed and adsorbed, further improving the antibacterial property of the fabric.
[0023] (2) The composite of graphene oxide, coupling agent and glycerol has a good effect on improving the anti-wrinkle performance of the fabric, making the fabric comfortable in stretchability and wrinkle resistance, and having excellent drape and feel.
[0024] (3) The preparation method of the present invention is simple, easy to operate, and suitable for industrial production. DETAILED DESCRIPTION
[0025] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with embodiments.
[0026] Example 1
[0027] A preparation process of an antibacterial and wrinkle-resistant fabric comprises the following steps:
[0028] M1: The fabric is added into a sodium hydroxide solution with a mass fraction of 5% for ultrasonic treatment and immersed for 1.5 hours before being taken out. The fabric is then ultrasonically washed with deionized water and dried to obtain the pretreated fabric for use;
[0029] M2: Mix nano zinc oxide, chitosan and cross-linking agent at room temperature to obtain mixed solution A, then add the pretreated fabric into the mixed solution A and stir, heat to 65°C and continue stirring for 4 hours. After the reaction, ultrasonically wash with deionized water and dry to constant weight.
[0030] M3: Add graphene oxide, coupling agent and glycerol into deionized water and mix and stir to obtain a mixed solution B, then place the fabric treated with M2 in the mixed solution B for immersion, and ultrasonically wash the fabric with deionized water, and finally dry it to constant weight to obtain the antibacterial and wrinkle-resistant fabric of the present invention.
[0031] The ultrasonic frequency is 70 Hz, and the ultrasonic time is 20 min.
[0032] The crosslinking agent in M2 is made of vinyltrimethylsilane and aminoformylhydrazide in a molar ratio of 1:5, and the preparation method is as follows:
[0033] Weigh a certain amount of aminoformyl hydrazide and water and add them into a reaction container, control the reaction container to be cooled to a constant temperature in an ice water bath, then add vinyltrimethylsilane dropwise into the reaction container, stir the reaction in an ice water bath for 30 minutes after the addition is complete, then heat the temperature to room temperature and stir the reaction for 2.5 hours, then perform reduced pressure distillation to obtain a cross-linking agent.
[0034] The stirring speed of M2 is 280 rpm, and the stirring time before heating is 15 min.
[0035] The particle size of the nano zinc oxide is 15 μm.
[0036] The mass ratio of the nano zinc oxide, chitosan and cross-linking agent is 3:4:5.5.
[0037] The padding time in the M3 is 2 h and the drying temperature is 60°C.
[0038] The mass ratio of the graphene oxide, the coupling agent, the glycerol and the water is 2:3:1.5:3, and the coupling agent is KH550.
[0039] An antibacterial and wrinkle-resistant fabric is prepared by the method.
[0040] The fabric is a knitted fabric.
[0041] Example 2
[0042] A preparation process of an antibacterial and wrinkle-resistant fabric comprises the following steps:
[0043] M1: The fabric is added into a sodium hydroxide solution with a mass fraction of 10% for ultrasonic treatment and immersed for 1.5 hours before being taken out. The fabric is then ultrasonically washed with deionized water and dried to obtain the pretreated fabric for use;
[0044] M2: Mix nano zinc oxide, chitosan and cross-linking agent at room temperature to obtain mixed solution A, then add the pretreated fabric into the mixed solution A and stir, heat to 70°C and continue stirring for 4 hours. After the reaction, ultrasonically wash with deionized water and dry to constant weight.
[0045] M3: Add graphene oxide, coupling agent and glycerol into deionized water and mix and stir to obtain a mixed solution B, then place the fabric treated with M2 in the mixed solution B for immersion, and ultrasonically wash the fabric with deionized water, and finally dry it to constant weight to obtain the antibacterial and wrinkle-resistant fabric of the present invention.
[0046] The ultrasonic frequency is 70 Hz, and the ultrasonic time is 30 min.
[0047] The crosslinking agent in M2 is made of vinyltrimethylsilane and aminoformylhydrazide in a molar ratio of 1:5, and the preparation method is as follows:
[0048] Weigh a certain amount of aminoformyl hydrazide and water and add them into a reaction container, control the reaction container to be cooled to a constant temperature in an ice water bath, then add vinyltrimethylsilane dropwise into the reaction container, stir the reaction in an ice water bath for 40 minutes after the addition is complete, then heat the temperature to room temperature and stir the reaction for 3 hours, then perform reduced pressure distillation to obtain a cross-linking agent.
[0049] The stirring speed in M2 is 300 rpm, and the stirring time before heating is 20 min.
[0050] The particle size of the nano zinc oxide is 10 μm.
[0051] The mass ratio of the nano zinc oxide, chitosan and cross-linking agent is 3:4:6.
[0052] The padding time in the M3 is 4 h and the drying temperature is 60°C.
[0053] The mass ratio of the graphene oxide, the coupling agent, the glycerol and the water is 2:3:1.5:3, and the coupling agent is KH550.
[0054] An antibacterial and wrinkle-resistant fabric is prepared by the method.
[0055] The fabric is a knitted fabric.
[0056] Example 3
[0057] A preparation process of an antibacterial and wrinkle-resistant fabric comprises the following steps:
[0058] M1: The fabric is added into a sodium hydroxide solution with a mass fraction of 10% for ultrasonic treatment and immersed for 1.5 hours before being taken out. The fabric is then ultrasonically washed with deionized water and dried to obtain the pretreated fabric for use;
[0059] M2: Mix nano zinc oxide, chitosan and cross-linking agent at room temperature to obtain mixed solution A, then add the pretreated fabric into the mixed solution A and stir, heat to 70°C and continue stirring for 6 hours. After the reaction, ultrasonically wash with deionized water and dry to constant weight.
[0060] M3: Add graphene oxide, coupling agent and glycerol into deionized water and mix and stir to obtain a mixed solution B, then place the fabric treated with M2 in the mixed solution B for immersion, and ultrasonically wash the fabric with deionized water, and finally dry it to constant weight to obtain the antibacterial and wrinkle-resistant fabric of the present invention.
[0061] The ultrasonic frequency is 70 Hz, and the ultrasonic time is 30 min.
[0062] The crosslinking agent in M2 is made of vinyltrimethylsilane and aminoformylhydrazide in a molar ratio of 1:5, and the preparation method is as follows:
[0063] Weigh a certain amount of aminoformyl hydrazide and water and add them into a reaction container, control the reaction container to be cooled to a constant temperature in an ice water bath, then add vinyltrimethylsilane dropwise into the reaction container, stir the reaction in an ice water bath for 40 minutes after the addition is complete, then heat the temperature to room temperature and stir the reaction for 3 hours, then perform reduced pressure distillation to obtain a cross-linking agent.
[0064] The stirring speed in the M2 is 300 rpm, and the stirring time before heating is 10 min.
[0065] The particle size of the nano zinc oxide is 10 μm.
[0066] The mass ratio of the nano zinc oxide, chitosan and cross-linking agent is 3:4:7.5.
[0067] The padding time in the M3 is 4 h and the drying temperature is 60°C.
[0068] The mass ratio of the graphene oxide, the coupling agent, the glycerol and the water is 2:2:1:2, and the coupling agent is KH550.
[0069] An antibacterial and wrinkle-resistant fabric is prepared by the method.
[0070] The fabric is a knitted fabric.
[0071] Example 4
[0072] A preparation process of an antibacterial and wrinkle-resistant fabric comprises the following steps:
[0073] M1: The fabric is added into a sodium hydroxide solution with a mass fraction of 5% for ultrasonic treatment and immersed for 1.5 hours before being taken out. The fabric is then ultrasonically washed with deionized water and dried to obtain the pretreated fabric for use;
[0074] M2: Mix nano zinc oxide, chitosan and cross-linking agent at room temperature to obtain mixed solution A, then add the pretreated fabric into the mixed solution A and stir, heat to 70°C and continue stirring for 6 hours. After the reaction, ultrasonically wash with deionized water and dry to constant weight.
[0075] M3: Add graphene oxide, coupling agent and glycerol into deionized water and mix and stir to obtain a mixed solution B, then place the fabric treated with M2 in the mixed solution B for immersion, and ultrasonically wash the fabric with deionized water, and finally dry it to constant weight to obtain the antibacterial and wrinkle-resistant fabric of the present invention.
[0076] The ultrasonic frequency is 70 Hz, and the ultrasonic time is 30 min.
[0077] The crosslinking agent in M2 is made of vinyltrimethylsilane and aminoformylhydrazide in a molar ratio of 1:5, and the preparation method is as follows:
[0078] Weigh a certain amount of aminoformyl hydrazide and water and add them into a reaction container, control the reaction container to be cooled to a constant temperature in an ice water bath, then add vinyltrimethylsilane dropwise into the reaction container, stir the reaction in an ice water bath for 40 minutes after the addition is complete, then heat the temperature to room temperature and stir the reaction for 3 hours, then perform reduced pressure distillation to obtain a cross-linking agent.
[0079] The stirring speed in M2 is 300 rpm, and the stirring time before heating is 20 min.
[0080] The particle size of the nano zinc oxide is 10 μm.
[0081] The mass ratio of the nano zinc oxide, chitosan and cross-linking agent is 3:4:5.
[0082] The padding time in the M3 is 4 h and the drying temperature is 60°C.
[0083] The mass ratio of the graphene oxide, the coupling agent, the glycerol and the water is 3:4:1.5:3, and the coupling agent is KH602.
[0084] An antibacterial and wrinkle-resistant fabric is prepared by the method.
[0085] The fabric is a knitted fabric.
[0086] Comparative Example 1
[0087] Based on Example 3, the cross-linking agent is aminocarbamoyl hydrazide.
[0088] Comparative Example 2
[0089] On the basis of Example 3, graphene oxide was replaced by an equal mass of glycerol.
[0090] Comparative Example 3
[0091] On the basis of Example 3, glycerol was replaced by an equal mass of graphene oxide.
[0092] Performance Test:
[0093] 1. Crease recovery angle test
[0094] Test materials: antibacterial and wrinkle-resistant fabrics prepared in Examples 1 to 4 and Comparative Examples 2 to 3.
[0095] Test method: Test according to GB / T 3819-1997 Determination of crease recovery of textile fabrics - Recovery angle method.
[0096] Test results: 6 batches of samples were tested according to the law, and the results are shown in Table 1.
[0097] Table 1 Wrinkle recovery angle (°) test results
[0098]
[0099] It can be seen from Table 1 that the wrinkle recovery angle test results of Examples 1 to 4 are better than those of Comparative Examples 2 to 3. The reason may be that the composite of graphene oxide, coupling agent, glycerol and deionized water has a good improvement effect on the wrinkle resistance of the fabric, thereby improving the wrinkle resistance of the fabric.
[0100] 2. Antibacterial test
[0101] Test materials: antibacterial and wrinkle-resistant fabrics prepared in Examples 1 to 4 and Comparative Example 1.
[0102] Test method: Test according to GB / T20944.2-2007 Evaluation of antimicrobial properties of textiles Part 2: Absorption method.
[0103] Test results: 5 batches of samples were tested according to the law, and the results are shown in Tables 2 to 4.
[0104] Table 2 Escherichia coli sterilization rate (%) test results
[0105]
[0106] Table 3 Staphylococcus aureus sterilization rate (%) test results
[0107]
[0108] Table 4 Klebsiella pneumoniae sterilization rate (%) test results
[0109]
[0110]
[0111] It can be seen from Tables 2 to 4 that the test results of the Escherichia coli sterilization rate, Staphylococcus aureus sterilization rate and Klebsiella pneumoniae sterilization rate of Examples 1 to 4 are better than those of Comparative Example 1. The reason may be that the cross-linking agent of the present invention can make the nano zinc oxide more uniformly adsorbed on the fabric, and the antibacterial property of the fabric is improved after the adsorption of nano zinc oxide and chitosan.
[0112] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A preparation process of an antibacterial and wrinkle-resistant fabric, characterized in that: The steps include: M1: Add the fabric into an alkali solution with a mass fraction of 5 to 10% for ultrasonic treatment and soak for 1 to 1.5 hours before taking it out. Then, the fabric is ultrasonically washed with deionized water and dried to obtain the pretreated fabric for use. M2: Mix nano zinc oxide, chitosan and cross-linking agent at room temperature to obtain mixed solution A, then add the pretreated fabric into the mixed solution A and stir, heat to 60-70°C and continue stirring for 4-6 hours. After the reaction, ultrasonically wash with deionized water and dry to constant weight. M3: Add graphene oxide, coupling agent and glycerol into deionized water and mix and stir to obtain a mixed solution B, then place the fabric treated with M2 in the mixed solution B for immersion, and ultrasonically wash the fabric with deionized water, and finally dry it to constant weight to obtain the antibacterial and wrinkle-resistant fabric of the present invention.
2. The preparation process of the antibacterial and wrinkle-resistant fabric according to claim 1, characterized in that: The ultrasonic frequency is 45-70 Hz, and the ultrasonic time is 20-30 min.
3. The preparation process of the antibacterial and wrinkle-resistant fabric according to claim 1, characterized in that: The crosslinking agent in M2 is made of vinyltrimethylsilane and aminoformylhydrazide in a molar ratio of 1:
5.
4. The process for preparing an antibacterial and wrinkle-resistant fabric according to claim 1, characterized in that: The stirring speed in the M2 is 220-300 rpm, and the stirring time before heating is 10-20 min.
5. The preparation process of the antibacterial and wrinkle-resistant fabric according to claim 1, characterized in that: The particle size of the nano zinc oxide is 10 to 20 μm.
6. The process for preparing an antibacterial and wrinkle-resistant fabric according to claim 1, characterized in that: The mass ratio of the nano zinc oxide, chitosan and cross-linking agent is 3:4:5-7.
5.
7. The process for preparing an antibacterial and wrinkle-resistant fabric according to claim 1, characterized in that: The padding time in the M3 is 2 to 4 hours, and the drying temperature is 45 to 60°C.
8. The process for preparing an antibacterial and wrinkle-resistant fabric according to claim 1, characterized in that: The mass ratio of the graphene oxide, the coupling agent, the glycerol and the deionized water is 2-3:3-5:1.5:3, and the coupling agent is any one of KH602, KH580 and KH550.
9. An antibacterial and wrinkle-resistant fabric, characterized in that: The fabric is prepared by the preparation process described in any one of claims 1 to 8.
10. The antibacterial and wrinkle-resistant fabric according to claim 1, characterized in that: The fabric is a knitted fabric.
Citation Information
Cited By
Environment-friendly antibacterial fabric and preparation method thereof
CN119932897A