Conductive silver paste for solar cell and solar cell

Through the silver powder and glass powder formula of specific morphology, the contact resistance and gate line resistance of solar cells are reduced, and the problem of high gate electrode resistance of existing solar cells is solved, achieving high aspect ratio gate electrode preparation and silver use savings.

CN119049759AActive Publication Date: 2024-11-29ZHEJIANG JINKO NEW MATERIAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411535683.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-30
Publication Date
2024-11-29
Estimated Expiration
2044-10-30

AI Technical Summary

Technical Problem

The gate electrode resistance of existing solar cells is high and has a large width, which cannot meet the development needs of new technologies.

Method used

The first silver powder and the second silver powder with a specific morphology are used to match the specific glass powder formula to reduce the softening temperature of the glass powder, reduce the sintering temperature through point-face contact, and form conductive silver paste with low contact resistance and gate line resistance. Used to prepare gate electrodes with a high aspect ratio.

Benefits of technology

Sintered at lower temperatures to form good ohmic contact, reduce contact resistance and gate line resistance, increase current, suitable for the preparation of fine gate printed screens, while saving silver usage and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119049759A_ABST
    Figure CN119049759A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of solar cells, in particular to conductive silver paste for a solar cell and the solar cell. The conductive silver paste comprises silver powder, glass powder, a carrier, an additive and a solvent, the silver powder comprises first silver powder particles and second silver powder particles; the first silver powder particle is in a sheet shape and comprises a first plane and a second plane which are opposite in the thickness direction, the average area of the first plane is recorded as S1, and the average area of the second plane is recorded as S2; the second silver powder particles are spherical-like, and the average equivalent particle size of the second silver powder particles is marked as D; s1, S2 and D meet the following conditions: 0.8 D < = S1 < = 2D, and 0.8 D < = S2 < = 2D; the glass powder comprises the following components by mole percent: 3%-10% of Na2CO3; 0.2%-1% of Al2O3; 1%-5% of SiO2; 1%-5% of ZnO; 30% to 50% of TeO2; 0.1%-2% of WO3; 20% to 40% of Pb3O4; 5%-10% of Bi2O3; 10%-20% of Li2CO3; 1% to 5% of B2O3; 0.05% to 0.5% of Fe2O3; and 0.05%-1.5% of CuO. The matched conductive paste can meet the printing requirement of a fine grid printing screen, a grid electrode with a high aspect ratio can be prepared, and meanwhile the conductivity is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of solar cells, and in particular to a conductive silver paste for solar cells and a solar cell. Background Art

[0002] Conductive silver paste includes high-temperature sintering silver paste and low-temperature curing silver paste. It is the key material for preparing solar cell electrodes. High-temperature sintering silver paste or low-temperature curing silver paste can be selected according to the needs of different types of solar cells. Taking high-temperature sintering silver paste as an example, it is usually composed of silver powder, glass powder, carrier and additives. Among them, the main function of the carrier is the wetting, printability, appearance and aspect ratio construction of the powder; the main function of the glass powder is to corrode the insulating silicon nitride anti-reflection film, help form ohmic contact and provide adhesion; the main function of silver powder is to act as a conductive medium, form electrode grid lines and provide a good conductive network; the main function of the additive is to improve the filling, printing, tension and other properties of the paste.

[0003] With the development of technology, higher requirements are placed on the resistance and width of the gate electrode of solar cells. Currently, the gate electrode prepared by conductive silver paste has high resistance and large width, which cannot adapt to the development of new technologies. Summary of the invention

[0004] Based on this, the first aspect of the present application provides a conductive silver paste for solar cells, and its technical solution is as follows:

[0005] A conductive silver paste comprises silver powder, glass powder, a carrier, an additive and a solvent;

[0006] The silver powder includes a first silver powder particle and a second silver powder particle; the first silver powder particle is in a flake shape, and along the thickness direction, the first silver powder particle includes a first plane and a second plane opposite to each other, and the average area of ​​the first plane is recorded as S1, and the unit is μm 2 The average area of ​​the second plane is recorded as S2, in μm 2 The second silver powder particles are spherical, and the average equivalent particle size of the second silver powder particles is recorded as D, in μm; S1, S2 and D satisfy: 0.8D≤S1≤2D, 0.8D≤S2≤2D;

[0007] The glass powder includes the following components in molar percentage:

[0008] Na2CO33%~10%;

[0009] Al2O30.2%~1%;

[0010] SiO21%~5%;

[0011] ZnO1%~5%;

[0012] TeO2 30%~50%;

[0013] WO30.1%~2%;

[0014] Pb3O420%~40%;

[0015] Bi2O35%~10%;

[0016] Li2CO310%~20%;

[0017] B2O31%~5%;

[0018] Fe2O30.05%~0.5%;

[0019] CuO0.05%~1.5%.

[0020] A second aspect of the present application provides a solar cell, which includes a gate electrode, wherein the gate electrode is made of the conductive silver paste for solar cells as described above.

[0021] Compared with the traditional solution, this application has the following beneficial effects:

[0022] Silver powder is the conductive functional phase in the conductive silver paste, which directly affects the conductive performance. The present application uses a first silver powder and a second silver powder with specific morphologies in combination, and matches them with a specific glass powder formula, wherein the Pb, W, Zn, Te, and Li elements in the glass powder can reduce the softening temperature of the glass powder, and the glass powder melts and releases heat, which can reduce the sintering temperature of the above-mentioned silver powder. When sintered at a lower temperature, there are a large number of point-to-surface contacts between the first silver powder and the second silver powder. After sintering, the contact resistance and the gate line resistance can be effectively reduced. The above-mentioned conductive silver paste can be used as a front silver paste in a crystalline silicon solar cell, and can form a good ohmic contact with a silicon substrate, form a good conductivity, effectively reduce the contact resistance and the gate line resistance, and increase the current. At the same time, the matched conductive paste can meet the printing requirements of a fine grid printing screen, and can prepare a gate electrode with a high aspect ratio, which is suitable for the preparation of a fine grid. At the same time, it can also save the use of silver and reduce costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the technical solutions in the embodiments of the present application and to more completely understand the present application and its beneficial effects, the following is a brief introduction to the drawings required for the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application, and those skilled in the art can obtain other drawings based on these drawings without creative work.

[0024] Figure 1 is a SEM image of a mixture of first silver powder particles and second silver powder particles according to one embodiment;

[0025] Figure 2 This is a SEM image of a comparison embodiment of a mixture of the third silver powder particles and the second silver powder particles. DETAILED DESCRIPTION

[0026] The present application will be further described in detail below in conjunction with specific embodiments. The present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present application more thoroughly understood.

[0027] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0028] the term

[0029] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:

[0030] In the present application, "plurality", "multiple", "multiple times", "plurality", etc., unless otherwise specified, refer to a number greater than 2 or equal to 2. For example, "one or more" means one or greater than or equal to two.

[0031] In this application, "optionally", "optional" and "optional" refer to optional, that is, to any one of the two parallel schemes of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent.

[0032] In this application, in the "first aspect", "second aspect", "third aspect", "fourth aspect", etc., the terms "first", "second", "third", "fourth", etc. are used only for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", "third", "fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.

[0033] In the present application, when it comes to numerical intervals (i.e., numerical ranges), unless otherwise specified, the optional numerical distribution is considered continuous within the above numerical interval, and includes the two numerical endpoints (i.e., the minimum and maximum values) of the numerical range, and each numerical value between the two numerical endpoints. Unless otherwise specified, when the numerical interval only refers to the integers within the numerical interval, it includes the two endpoint integers of the numerical range, and each integer between the two endpoints. In this article, it is equivalent to directly listing each integer, such as t is an integer selected from 1 to 10, indicating that t is any integer selected from the integer group consisting of 1, 2, 3, 4, 5, 6, 7, 8, 9 and 10. In addition, when multiple ranges are provided to describe features or characteristics, these ranges can be combined. In other words, unless otherwise specified, the ranges disclosed herein should be understood to include any and all sub-ranges included therein.

[0034] The temperature parameters in this application, unless otherwise specified, are allowed to be either constant temperature treatment or to vary within a certain temperature range. It should be understood that the constant temperature treatment allows the temperature to fluctuate within the accuracy range controlled by the instrument. Fluctuations within the range of ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are allowed.

[0035] In the present application, the percentage content, unless otherwise specified, refers to mass percentage for solid-liquid mixing and solid-solid mixing, and volume percentage for liquid-liquid mixing.

[0036] In this application, when it comes to percentage concentration, unless otherwise specified, it refers to the final concentration. The final concentration refers to the proportion of the added component in the system after the addition of the component.

[0037] In the present application, %(w / w) and wt% both represent weight percentage, %(v / v) refers to volume percentage, and %(w / v) refers to mass volume percentage.

[0038] The average equivalent particle size of the present invention can be tested by a laser particle size analyzer.

[0039] In a first aspect, the present application provides a conductive silver paste for solar cells. In one embodiment, the conductive silver paste includes silver powder, glass powder, a carrier, an additive and a solvent;

[0040] The silver powder includes a first silver powder particle and a second silver powder particle; the first silver powder particle is in a flake shape, and along the thickness direction, the first silver powder particle includes a first plane and a second plane opposite to each other, and the average area of ​​the first plane is recorded as S1, and the unit is μm 2 The average area of ​​the second plane is recorded as S2, in μm 2The second silver powder particles are spherical, and the average equivalent particle size of the second silver powder particles is recorded as D, in μm; S1, S2 and D satisfy: 0.8D≤S1≤2D, 0.8D≤S2≤2D;

[0041] The glass powder includes the following components in molar percentage:

[0042] Na2CO33%~10%;

[0043] Al2O30.2%~1%;

[0044] SiO21%~5%;

[0045] ZnO1%~5%;

[0046] TeO2 30%~50%;

[0047] WO30.1%~2%;

[0048] Pb3O420%~40%;

[0049] Bi2O35%~10%;

[0050] Li2CO310%~20%;

[0051] B2O31%~5%;

[0052] Fe2O30.05%~0.5%;

[0053] CuO0.05%~1.5%.

[0054] Silver powder is the conductive functional phase in the conductive silver paste, which directly affects the conductive performance. The present application uses a first silver powder and a second silver powder with specific morphologies in combination, and matches them with a specific glass powder formula, wherein the Pb, W, Zn, Te, and Li elements in the glass powder can reduce the softening temperature of the glass powder, and the glass powder melts and releases heat, which can reduce the sintering temperature of the above-mentioned silver powder. When sintered at a lower temperature, there are a large number of point-to-surface contacts between the first silver powder and the second silver powder. After sintering, the contact resistance and the gate line resistance can be effectively reduced. The above-mentioned conductive silver paste can be used as a front silver paste in a crystalline silicon solar cell, and can form a good ohmic contact with a silicon substrate, form a good conductivity, effectively reduce the contact resistance and the gate line resistance, and increase the current. At the same time, the matched conductive paste can meet the printing requirements of a fine grid printing screen, and can prepare a gate electrode with a high aspect ratio, which is suitable for the preparation of a fine grid. At the same time, it can also save the use of silver and reduce costs.

[0055] The first silver powder particles are in the form of flakes, and the contact between the particles is a mixed mode of surface contact, line contact, and point contact. The contact area in the conductive network is sufficient, and it can have very low contact resistance and grid line resistance, so the conductive performance is excellent. At the same time, the flake silver powder can reduce the amount of the second spherical silver powder particles used in combination. Under the premise of ensuring conductivity, the amount of silver powder used in the production process can be effectively reduced, and the cost can be reduced. However, the important problem faced by the use of flake silver powder is that it is difficult to adapt to the printing requirements of fine grid screens. The present application overcomes the above problem by controlling S1, S2 and D, and the conductive silver paste formed can be used for printing to form fine grid lines.

[0056] Optionally, the S1 is at 0.8 μm 2 ~2μm 2 For example, S1 is 0.8 μm 2 , 1μm 2 , 1.2μm 2 , 1.4μm 2 , 1.6μm 2 , 1.8μm 2 , 2μm 2 .

[0057] Optionally, the circularity of the first plane is in the range of 0.5 to 1. For example, the circularity of the first plane is 0.5, 0.6, 0.7, 0.8, 0.9, 1. The circularity of the first plane refers to the degree of proximity between the orthographic projection of the first plane of the particle and the circle, which can be expressed by the formula: e1=(4π×orthographic projection area) / (perimeter×perimeter), where e1 is the circularity of the first plane. When e1=1, the first plane of the particle is a circle, and the smaller e is, the greater the difference between the first plane and the circle.

[0058] Optionally, the first plane has a plurality of straight edges, and two adjacent straight edges are smoothly connected. Two adjacent straight edges are smoothly connected to form a chamfer.

[0059] Optionally, the first plane with three straight edges accounts for 5% to 10% of the total number of first planes of the first silver powder particles. For example, the first plane with three straight edges accounts for 5%, 6%, 7%, 8%, 9%, and 10% of the total number of first planes of the first silver powder particles. There are more particles with triangular chamfered morphology, which is conducive to lower resistance of the slurry line and better conductivity.

[0060] Optionally, the S2 is at 0.8 μm 2 ~2μm 2 For example, S2 is 0.8 μm 2 , 1μm 2 , 1.2μm 2 , 1.4μm 2 , 1.6μm2 , 1.8μm 2 , 2μm 2 .

[0061] Optionally, the circularity of the second plane is in the range of 0.5 to 1. For example, the circularity of the second plane is 0.5, 0.6, 0.7, 0.8, 0.9, 1. The circularity of the second plane refers to the degree of proximity between the orthographic projection of the second plane of the particle and the circle, which can be expressed by the formula: e2=(4π×orthographic projection area) / (perimeter×perimeter), where e2 is the circularity of the first plane. When e2=1, the second plane of the particle is a circle, and the smaller e is, the greater the difference between the first plane and the circle is.

[0062] Optionally, the second plane has a plurality of straight edges, and two adjacent straight edges are smoothly connected. Two adjacent straight edges are smoothly connected to form a chamfer.

[0063] Optionally, the second plane with three straight edges accounts for 5% to 10% of the total number of second planes of the first silver powder particles. For example, the second plane with three straight edges accounts for 5%, 6%, 7%, 8%, 9%, and 10% of the total number of second planes of the first silver powder particles. There are more particles with triangular chamfered morphology, which is conducive to lower resistance of the slurry line and better conductivity.

[0064] Optionally, the average equivalent particle size of the first silver powder particles is 0.5 μm to 1.6 μm. For example, the average equivalent particle size of the first silver powder particles is 0.5 μm, 0.7 μm, 0.9 μm, 1 μm, 1.2 μm, 1.4 μm, and 1.6 μm. Compared with the general flaky particle size of more than 2 μm, the particle size of the first silver powder is smaller.

[0065] Optionally, D is in the range of 0.4 μm to 1 μm. For example, D is 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, or 1 μm.

[0066] Optionally, the sphericity of the second silver powder particles is 60% to 80%. For example, the sphericity of the second silver powder particles is 60%, 70%, or 80%.

[0067] Optionally, the specific surface area of ​​the second silver powder is in the range of 0.6 g / mL to 0.9 g / mL. For example, the specific surface area of ​​the second silver powder is 0.6 g / mL, 0.7 g / mL, 0.8 g / mL, or 0.9 g / mL.

[0068] The first silver powder and the second silver powder can be commercially available.

[0069] Optionally, the mass ratio of the first silver powder particles to the second silver powder particles is 1:(1.5-5). For example, the mass ratio of the first silver powder particles to the second silver powder particles is 1:1.5, 1:2, 1:3, 1:4, 1:5.

[0070] Optionally, the melting point of the first silver powder particles is higher than the melting point of the second silver powder particles.

[0071] Optionally, the mass proportion of the silver powder in the conductive silver paste is 86% to 96%. For example, the mass proportion of the silver powder in the conductive silver paste is 86%, 90%, 91%, 93%, or 96%.

[0072] At the same time, when the above-mentioned silver powder is combined with specific glass powder, the conductive silver paste can effectively reduce the contact resistance and gate line resistance.

[0073] In the glass powder, the molar percentage of Na2CO3 includes but is not limited to 3%, 5%, 7%, 9%, and 10%; the molar percentage of Al2O3 includes but is not limited to 0.2%, 0.5%, and 1%; the molar percentage of SiO2 includes but is not limited to 1%, 3%, and 5%; the molar percentage of ZnO includes but is not limited to 1%, 3%, and 5%; the molar percentage of TeO2 includes but is not limited to 30%, 40%, and 50%; the molar percentage of WO3 includes but is not limited to 0.1%, 0.5%, 1%, and 2%; the molar percentage of Pb3O4 includes but is not limited to 20%, 30%, and 40%; the molar percentage of Bi2O3 includes but is not limited to 5%, 8%, and 10%; the molar percentage of Li2CO3 includes but is not limited to 10%, 15%, and 20%; the molar percentage of B2O3 includes but is not limited to 1%, 3%, and 5%; the molar percentage of Fe2O3 includes but is not limited to 0.05%, 0.1%, 0.3%, and 0.5%; the molar percentage of CuO includes but is not limited to 0.05%, 1%, 0.5%, 1%, and 1.5%.

[0074] Optionally, the glass powder accounts for 1% to 3% by mass in the conductive silver paste. For example, the glass powder accounts for 1%, 2%, or 3% by mass in the conductive silver paste.

[0075] Optionally, the carrier is selected from one or more of dibutyl phthalate, dimethyl oxalate and hydrogenated rosin pentaerythritol ester.

[0076] Optionally, the mass proportion of the carrier in the conductive silver paste is 1% to 5%. For example, the mass proportion of the carrier in the conductive silver paste is 1%, 3%, or 5%.

[0077] Optionally, the additive is selected from one or more of ethyl cellulose, hydrogenated castor oil, polyamide wax, polyvinyl alcohol and metal soap.

[0078] Optionally, the additive accounts for 1.5% to 6% by weight of the conductive silver paste. For example, the additive accounts for 1.5%, 2%, 3%, 4%, or 6% by weight of the conductive silver paste.

[0079] Optionally, the solvent is selected from one or more of dodecyl alcohol ester, hexadecanol ester, diethylene glycol butyl ether acetate, tripropylene glycol butyl ether, diethylene glycol monobutyl ether and diethylene glycol dibutyl ether.

[0080] Optionally, the mass proportion of the solvent in the conductive silver paste is 0.5% to 1.5%. For example, the mass proportion of the solvent in the conductive silver paste is 0.5%, 1%, or 1.5%.

[0081] A second aspect of the present application provides a solar cell, which includes a gate electrode, wherein the gate electrode is prepared from the above-mentioned conductive silver paste.

[0082] The following is further described in conjunction with specific embodiments and comparative examples. The raw materials involved in the following specific embodiments and comparative examples, unless otherwise specified, can all be commercially available, the instruments used, unless otherwise specified, can all be commercially available, and the processes involved, unless otherwise specified, are all routinely selected by those skilled in the art.

[0083] The first silver powder is of the brand FD-3 purchased from Jiangxi Beiteli New Materials Co., Ltd., and the second silver powder is of the brand 814B purchased from Shenzhen Hashen Intelligent Materials Co., Ltd. The first silver powder and the second silver powder are mixed at a mass ratio of 1:5. The SEM image of the mixed powder is as follows: Figure 1 As shown. Figure 1 It can be seen that the first silver powder particles 11 are in the form of flakes. Along the thickness direction, each first silver powder particle includes a first plane and a second plane. The average area of ​​the first plane is recorded as S1, and the unit is μm. 2 The average area of ​​the second plane is recorded as S2, in μm 2 , S1 at 1.2μm 2 The first plane has a circularity of about 0.5 to 1, has a plurality of straight edges, two adjacent straight edges are smoothly connected, and the first plane with three straight edges accounts for 5% to 10% of the total number of first planes of the first silver powder particles. S2 is 1.2 μm. 2The second plane has a circularity of about 0.5 to 1, the second plane has a plurality of straight edges, two adjacent straight edges are smoothly connected, and the second plane with three straight edges accounts for 5% to 10% of the total number of second planes of the first silver powder particles. The second silver powder particles are spherical, and the average equivalent particle size of the second silver powder particles is D, which is about 1.2 μm.

[0084] The third silver powder is 708B, purchased from Shenzhen Ha Shen Zhi Cai Co., Ltd. The third silver powder is mixed with the second silver powder at a mass ratio of 1:5. The SEM image of the mixed powder is as follows: Figure 2 As shown. Figure 2 It can be seen that the third silver powder 13 is in the form of flakes. Along the thickness direction, each third silver powder particle includes an average area relative to the first plane and the second plane, and the average area of ​​the first plane is recorded as S1, in μm. 2 The average area of ​​the second plane is recorded as S2, in μm 2 , S1 at 5μm 2 Around, S2 at 5μm 2 about.

[0085] Example 1

[0086] The present embodiment provides a conductive silver paste, and the preparation method thereof is as follows: according to the mass ratio shown in Table 1, a first silver powder, a second silver powder, a glass powder, dibutyl phthalate (carrier), dodecyl alcohol ester (solvent) and ethyl cellulose (additive) are mixed, and stirred evenly to obtain a conductive silver paste, wherein the preparation method of the glass powder is as follows: the components and their molar percentages shown in Table 2 are mixed.

[0087] Example 2

[0088] The present embodiment provides a conductive silver paste, and the preparation method thereof is as follows: according to the mass ratio shown in Table 1, a first silver powder, a second silver powder, a glass powder, dimethyl oxalate (carrier), hexadecanol ester (solvent) and hydrogenated castor oil (additive) are mixed, and stirred evenly to obtain a conductive silver paste, wherein the preparation method of the glass powder is the same as that in Example 1.

[0089] Example 3

[0090] The present embodiment provides a conductive silver paste, and the preparation method thereof is as follows: according to the mass ratio shown in Table 1, a first silver powder, a second silver powder, a glass powder, hydrogenated rosin pentaerythritol ester (carrier), diethylene glycol butyl ether acetate (solvent) and polyamide wax (additive) are mixed, and stirred evenly to obtain a conductive silver paste, wherein the preparation method of the glass powder is the same as that in Example 1.

[0091] Example 4

[0092] The present embodiment provides a conductive silver paste, and the preparation method thereof is as follows: according to the mass ratio shown in Table 1, a first silver powder, a second silver powder, a glass powder, dibutyl phthalate (carrier), tripropylene glycol butyl ether (solvent) and polyvinyl alcohol (additive) are mixed, and stirred evenly to obtain a conductive silver paste, wherein the preparation method of the glass powder is the same as that in Example 1.

[0093] Example 5

[0094] The present embodiment provides a conductive silver paste, and the preparation method thereof is as follows: according to the mass ratio shown in Table 1, a first silver powder, a second silver powder, a glass powder, dibutyl phthalate (carrier), diethylene glycol monobutyl ether (solvent) and a metal soap (additive) are mixed, and stirred evenly to obtain a conductive silver paste, wherein the preparation method of the glass powder is the same as that in Example 1.

[0095] Example 6

[0096] The present embodiment provides a conductive silver paste, and the preparation method thereof is as follows: according to the mass ratio shown in Table 1, a first silver powder, a second silver powder, a glass powder, dibutyl phthalate (carrier), dodecyl alcohol ester (solvent) and ethyl cellulose (additive) are mixed, and stirred evenly to obtain a conductive silver paste, wherein the preparation method of the glass powder is as follows: the components and their molar percentages shown in Table 2 are mixed.

[0097] Example 7

[0098] The present embodiment provides a conductive silver paste, and the preparation method thereof is as follows: according to the mass ratio shown in Table 1, a first silver powder, a second silver powder, a glass powder, dibutyl phthalate (carrier), dodecyl alcohol ester (solvent) and ethyl cellulose (additive) are mixed, and stirred evenly to obtain a conductive silver paste, wherein the preparation method of the glass powder is as follows: the components and their molar percentages shown in Table 2 are mixed.

[0099] Example 8

[0100] The present embodiment provides a conductive silver paste, and the preparation method thereof is as follows: according to the mass ratio shown in Table 1, a first silver powder, a second silver powder, a glass powder, dibutyl phthalate (carrier), dodecyl alcohol ester (solvent) and ethyl cellulose (additive) are mixed, and stirred evenly to obtain a conductive silver paste, wherein the preparation method of the glass powder is as follows: the components and their molar percentages shown in Table 2 are mixed.

[0101] Example 9

[0102] The present embodiment provides a conductive silver paste, and the preparation method thereof is as follows: according to the mass ratio shown in Table 1, a first silver powder, a second silver powder, a glass powder, dibutyl phthalate (carrier), dodecyl alcohol ester (solvent) and ethyl cellulose (additive) are mixed, and stirred evenly to obtain a conductive silver paste, wherein the preparation method of the glass powder is as follows: the components and their molar percentages shown in Table 2 are mixed.

[0103] Comparative Example 1

[0104] This comparative example provides a conductive silver paste, and the preparation method thereof is as follows: according to the mass ratio shown in Table 1, a third silver powder, a second silver powder, a glass powder, dibutyl phthalate (carrier), dodecyl alcohol ester (solvent) and ethyl cellulose (additive) are mixed, and stirred evenly to obtain a conductive silver paste, wherein the preparation method of the glass powder is the same as that in Example 1.

[0105] Comparative Example 2

[0106] The present comparative example provides a conductive silver paste, and the preparation method thereof is as follows: according to the mass ratio shown in Table 1, a first silver powder, a second silver powder, a glass powder, dibutyl phthalate (carrier), dodecyl alcohol ester (solvent) and ethyl cellulose (additive) are mixed, and stirred evenly to obtain a conductive silver paste, wherein the preparation method of the glass powder is as follows: the components and their molar percentages shown in Table 2 are mixed.

[0107] The formulas of the conductive silver pastes of the embodiments and comparative examples are summarized in Table 1.

[0108] Table 1

[0109]

[0110] Table 2

[0111]

[0112] test

[0113] The conductive silver paste of each embodiment and comparative example was printed onto a battery substrate and subjected to the same sintering conditions to form a gate electrode of the same circuit. The aspect ratio of the gate electrode is shown in Table 3. The conductivity of the gate electrode was tested by a TLM contact resistance tester, and the results are shown in Table 3.

[0114] Table 3

[0115]

[0116] It can be seen from the above table that in Examples 1 to 9, when the first silver powder, the second silver powder, the glass powder and other reagents are added to the conductive silver paste, the gate electrode prepared by printing can have a higher aspect ratio, can meet the printing requirements of fine gates, and at the same time has a lower line resistance, providing good conductivity.

[0117] According to the comparison between Comparative Example 1 and Example 5, the combination of the first silver powder and the second silver powder is more conducive to preparing a gate electrode with a high aspect ratio, and the gate electrode has a lower resistance, which indicates that the morphology of the silver powder affects the conductivity and processability of the conductive silver paste.

[0118] According to the comparison between Comparative Example 2 and Example 5, the composition of the glass powder affects the conductivity and processability of the conductive silver paste. By combining the glass powder with the first silver powder and the second silver powder in a specific ratio and composition, the conductivity of the conductive silver paste is improved and a gate electrode with a high aspect ratio is obtained.

[0119] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0120] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be subject to the attached claims.

Claims

1. A conductive silver paste for solar cells, characterized in that: Including silver powder, glass powder, carrier, additive and solvent; The silver powder includes a first silver powder particle and a second silver powder particle; the first silver powder particle is in a flake shape, and along the thickness direction, the first silver powder particle includes a first plane and a second plane opposite to each other, and the average area of ​​the first plane is recorded as S1, and the unit is μm 2 The average area of ​​the second plane is recorded as S2, in μm 2 The second silver powder particles are spherical, and the average equivalent particle size of the second silver powder particles is recorded as D, in μm; S1, S2 and D satisfy: 0.8D≤S1≤2D, 0.8D≤S2≤2D; The glass powder includes the following components in molar percentage: Na2CO33%~10%; Al2O30.2%~1%; SiO21%~5%; ZnO1%~5%; TeO2 30%~50%; WO30.1%~2%; Pb3O420%~40%; Bi2O35%~10%; Li2CO310%~20%; B2O31%~5%; Fe2O30.05%~0.5%; CuO0.05%~1.5%.

2. The conductive silver paste for solar cells according to claim 1, characterized in that: At least one of the following conditions is met: (1) S1 at 0.8 μm 2 ~2μm 2 within the scope; (2) S2 at 0.8 μm 2 ~2μm 2 within the scope; (3) The D is in the range of 0.4 μm to 1 μm.

3. The conductive silver paste for solar cells according to claim 1, characterized in that: Includes at least one of the following features: (1) The circularity of the first plane is in the range of 0.5 to 1; (2) The circularity of the second plane is in the range of 0.5 to 1.

4. The conductive silver paste for solar cells according to claim 3, characterized in that: Includes at least one of the following features: (1) The first plane has a plurality of straight edges, and two adjacent straight edges are smoothly connected; (2) The second plane has a plurality of straight edges, and two adjacent straight edges are smoothly connected.

5. The conductive silver paste for solar cells according to claim 4, characterized in that: Includes at least one of the following features: (1) The first plane having three straight edges accounts for 5% to 10% of the total number of first planes of the first silver powder particles; (2) The second planes having three straight edges account for 5% to 10% of the total number of the second planes of the first silver powder particles.

6. The conductive silver paste for solar cells according to claim 1, characterized in that: The sphericity of the second silver powder particles is 60% to 80%.

7. The conductive silver paste for solar cells according to claim 1, characterized in that: The specific surface area of ​​the second silver powder is in the range of 0.6 g / mL to 0.9 g / mL.

8. The conductive silver paste for solar cells according to any one of claims 1 to 7, characterized in that: Includes at least one of the following features: (1) The mass ratio of the first silver powder particles to the second silver powder particles is 1:(1.5-5); (2) The melting point of the first silver powder particles is higher than the melting point of the second silver powder particles.

9. The conductive silver paste for solar cells according to any one of claims 1 to 7, characterized in that: Includes at least one of the following features: (1) The mass proportion of the silver powder in the conductive silver paste is 86% to 96%; (2) The mass proportion of the glass powder in the conductive silver paste is 1% to 3%; (3) The mass proportion of the carrier in the conductive silver paste is 1% to 5%; (4) The carrier is selected from one or more of dibutyl phthalate, dimethyl oxalate and hydrogenated rosin pentaerythritol ester; (5) The mass proportion of the additive in the conductive silver paste is 1.5% to 6%; (6) The additive is selected from one or more of ethyl cellulose, hydrogenated castor oil, polyamide wax, polyvinyl alcohol and metal soap; (7) The mass proportion of the solvent in the conductive silver paste is 0.5% to 1.5%; (8) The solvent is selected from one or more of dodecyl alcohol ester, hexadecanol ester, diethylene glycol butyl ether acetate, tripropylene glycol butyl ether, diethylene glycol monobutyl ether and diethylene glycol dibutyl ether.

10. A solar cell, characterized in that: The invention comprises a gate electrode, wherein the gate electrode is prepared from the conductive silver paste for solar cells according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Silicon solar cell front face electrode silver paste and preparing method thereof

    CN104157328A

  • Heterojunction solar cell conductive silver paste and low-temperature curing method thereof

    CN111341482A

  • Solar cell anode conductive silver paste and preparation method thereof

    CN111540500A

  • Conductive composition, manufacturing method of solar cell using it, and solar cell

    JP2012074655A

  • Glass frit, preparation method therefor and electrode paste containing glass frit

    WO2016169512A1