High-surface-capacity lithium metal solid-state battery and preparation method thereof

Through in-situ polymerization technology, a multi-phase ion transmission channel of high-permeability precursor solution and active filler is constructed, which solves the problems of poor contact between solid electrolytes and electrodes of lithium-ion batteries and low ion conductivity, and achieves high load positive electrodes and integrated The preparation of chemical batteries improves the surface capacity and cycle life of the battery, and reduces cost and environmental impact.

CN119050490AInactive Publication Date: 2024-11-29广东鹏锦智能装备股份有限公司

Patent Information

Application Number
CN202411168400.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

There are problems of physical contact differences and low ion conductivity between the solid electrolytes and electrodes of traditional lithium-ion batteries, and the solution preparation process is complex and not environmentally friendly, resulting in battery safety risks and high costs.

Method used

Using in-situ polymerization technology, a multiphase ion transport channel is constructed through highly permeable precursor solutions and active fillers, and a high-load positive electrode and integrated "electrode/electrolyte" are prepared to improve the ion conductivity of the battery and the active substances inside the electrode. Availability to avoid electrode cracking and solvent waste.

Benefits of technology

A solid electrolyte with high conductivity and high migration number at room temperature is achieved, which enhances the electrode/electrolyte interface, improves the surface capacity and cycle life of lithium metal batteries, and reduces cost and environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050490A_ABST
    Figure CN119050490A_ABST
Patent Text Reader

Abstract

The invention provides a high-surface-capacity lithium metal solid-state battery and a preparation method thereof, and belongs to the technical field of lithium batteries. Comprising the following steps: S1, uniformly stirring and mixing a lithium salt, a polymer monomer, a thickening agent and a cross-linking agent to obtain a precursor solution; s2, blending and stirring the precursor solution with a nanoscale active filler and a free radical initiator to obtain a thick composite liquid electrolyte, and carrying out thermal polymerization on the composite liquid electrolyte to obtain a composite solid electrolyte; s3, adding a conductive agent, a nanoscale positive electrode material and a free radical initiator into the precursor solution, stirring and blending, pouring the mixture into an aluminum foil, and performing thermal polymerization to obtain a positive electrode; and S4, dropping a composite liquid electrolyte on the positive electrode, heating, assembling the battery with a lithium negative electrode, heating and standing to obtain the high-surface-capacity lithium metal solid-state battery. Through in-situ polymerization, an ion transmission channel in the electrode is additionally increased, and active substances in the electrode are fully utilized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium batteries, and in particular to a high-area capacity lithium metal solid-state battery and a preparation method thereof. Background Art

[0002] Traditional lithium-ion batteries use organic liquid electrolytes with low flash points, which pose great safety hazards during use. To this end, the power battery vehicle industry is working hard to promote high-performance solid electrolytes to improve battery safety performance. However, traditional solid electrolytes are prepared separately and stacked with positive and negative electrodes to form batteries. This non-in-situ preparation process (patent CN202111482846.X) will undoubtedly lead to incompatible solid / solid interfaces and low ion conductivity. Through in-situ polymerization, not only can the inside of the electrode be fully wetted by the polymer monomer precursor solution to solve problems such as poor physical contact between the electrode and the electrolyte, but also the traditional solution method (patent CN202110463439.8) is abandoned. The complex processes such as dissolution and drying film formation caused by the preparation of polymer-based solid electrolytes effectively reduce costs.

[0003] In recent years, conventional in-situ polymer systems are represented by glass fiber and diaphragm-assisted methods (patent CN117229447B), which inject polymerizable monomer precursors into the battery diaphragm and then thermally polymerize in the battery. However, since the diaphragm itself is an ion-conducting inert material and cannot transmit lithium ions, this method will sacrifice some ion conductivity, but it provides feasibility for the development of diaphragm-free solid electrolyte preparation technology research with excellent interface properties and high ion conductivity, and also lays the foundation for the construction of "electrode / electrolyte" integrated solid-state batteries.

[0004] At present, the traditional method has the following problems:

[0005] (i) Most of the separately prepared solid electrolytes have problems such as poor physical contact with electrodes and low ion conductivity, and the solution method preparation process will produce a large number of complex solvent treatment processes and solvent waste. Therefore, the solid-state battery prepared by the in-situ polymerization method proposed in the present invention is not only conducive to solving the interface problem between the electrolyte and the electrode and the ion conduction problem, but also abandons the complex processes such as dissolution and drying film formation caused by the solution method, effectively improving the utilization rate of raw materials, being environmentally friendly, and reducing costs.

[0006] (ii) The in-situ polymerization technology used in the present invention does not use ion-conducting inert materials such as glass fibers and diaphragms as self-supporting structures, which better ensures the ion transport inside the electrolyte; in addition, the active filler used can not only serve as a self-supporting structure, but also construct a variety of ion conduction channels to ensure high ionic conductivity of the electrolyte.

[0007] (III) The preparation of conventional positive electrodes uses polymer binders, which are prone to cracking during the high-temperature drying process of preparing thick electrodes. The high-load positive electrode prepared by the present invention does not require drying, thereby avoiding electrode cracking.

[0008] (iv) The high-load electrode prepared by the traditional wet method has poor conductivity during the charge and discharge process, and the capacity of the active material is difficult to fully utilize. The present invention increases the internal ion transmission channel of the electrode through in-situ polymerization, and fully utilizes the active material inside the electrode.

[0009] In addition, the high-load cathode prepared by the common coating method has poor conductivity, and the active materials inside the electrode basically do not participate in the Faraday reaction, which further limits the improvement of the battery surface capacity. Therefore, the development of high-energy-density solid-state batteries requires the construction of a high-load cathode with multiple ion transport channels. Summary of the invention

[0010] In order to overcome the shortcomings of the prior art, the present invention proposes a method and application of in-situ polymerization to prepare a solid electrolyte, a high-load positive electrode, an integrated "electrode / electrolyte" and a high-areal capacity lithium metal solid-state battery.

[0011] The technical solution of the present invention is achieved in this way:

[0012] The first purpose of the present invention is to propose a method for preparing an in-situ polymerized solid electrolyte, which solves the problem of poor physical contact between the electrode and the electrolyte through the highly permeable precursor solution, and through the addition of active fillers, it not only serves as a self-supporting structure, but also constructs a multiphase ion transport channel, including polymer phase ion conduction and organic-inorganic phase interface ion conduction, solves the problem of low ion conductivity of the solid electrolyte, and ensures its normal operation at room temperature.

[0013] The second purpose of the present invention is to propose a method for preparing a high-load positive electrode by in-situ polymerization to solve the cracking problem that occurs when preparing a high-load electrode by a wet method. In addition, in addition to the internal lattice transmission of lithium ions in the positive electrode material, an additional ion transmission channel is constructed inside the electrode through the lithium salt of the precursor solution.

[0014] The third purpose of the present invention is to propose a method for constructing an integrated "electrode / electrolyte" by in-situ polymerization, and apply it in solid-state batteries, providing technical support for the design of high-area capacity batteries.

[0015] The purpose of the present invention is achieved by at least one of the following technical solutions.

[0016] The in-situ polymerization method for constructing an integrated high-area capacity lithium metal solid-state battery provided by the present invention specifically comprises the following steps:

[0017] S1. The lithium salt, polymer monomer, thickener and crosslinking agent are stirred and mixed to obtain a uniform precursor solution;

[0018] S2. The precursor solution is blended and stirred with a nanoscale active filler and a free radical initiator to obtain a thick composite liquid electrolyte, and the composite liquid electrolyte is subjected to thermal polymerization to obtain a composite solid electrolyte;

[0019] S3. Adding a conductive agent, a nanoscale cathode material and a free radical initiator to the precursor solution, stirring and blending, pouring the mixture into an aluminum foil, and thermally polymerizing to obtain a cathode;

[0020] S4. dripping a composite liquid electrolyte onto the positive electrode, heating it, assembling a battery with a lithium negative electrode, heating and allowing it to stand, to obtain a high surface capacity lithium metal solid-state battery.

[0021] Further, the lithium salt concentration is 0.2-1.5 mol / L;

[0022] The volume proportion of the polymer monomer is 4-30 vol%;

[0023] The volume fraction of the thickener is 60-95 vol%;

[0024] The volume fraction of the cross-linking agent is 1-10 vol%;

[0025] The mass fraction of the nano-scale active filler is 5-60%;

[0026] The mass fraction of the free radical initiator is 0.2-5%;

[0027] The mass fraction of the precursor solution in the high-load positive electrode is 2-10%;

[0028] The mass fraction of the conductive agent is 2-10%;

[0029] The mass fraction of the nano-scale positive electrode material is 70-95%.

[0030] Further, the lithium salt is one or more of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium nitrate (LiNO3), lithium difluorooxalatoborate (LiDFOB), and lithium difluorophosphate (LiPO2F2);

[0031] Preferably, the lithium salt is a single salt of lithium bis(trifluoromethanesulfonyl imide); or the lithium salt is a combined lithium salt of lithium bis(trifluoromethanesulfonyl imide) and lithium nitrate, and the mass ratio of the two is 10:1, and the lithium salt concentration in the preparation of the precursor solution is 1 mol / L.

[0032] Furthermore, the polymer monomer is one or more of butyl acrylate, polyethylene glycol diacrylate, ethyl cyanoacrylate, and trifluoroethyl methacrylate.

[0033] Preferably, the polymer monomer is trifluoroethyl methacrylate, and the volume fraction is 20 vol%.

[0034] Furthermore, the thickener is one or more of ethylene carbonate (EC), fluoroethylene carbonate (FEC), vinylene carbonate (VC), and succinonitrile (SN).

[0035] Preferably, the thickener is fluoroethylene carbonate (FEC), and the mass fraction of the thickener in the preparation of the precursor solution is about 79 vol%.

[0036] Furthermore, the cross-linking agent is one or more of methacrylate, pentaerythritol tetraacrylate, propylene glycol acrylate, and glycerol acrylate;

[0037] Preferably, the crosslinking agent is pentaerythritol tetraacrylate, and the mass fraction of the crosslinking agent in the preparation of the precursor solution is 1%.

[0038] Furthermore, the nano active filler is garnet-type Li 3+x A3B2O 12 Oxide (LLZTO), sulfide (Li 10 GeP2S 12 and Li6PS5Cl), lithium iron phosphate, lithium nickel cobalt manganese oxide, and lithium cobalt oxide.

[0039] Preferably, the nano-active filler is lithium iron phosphate, and the mass ratio of the nano-active filler to the precursor solution is 1:4.

[0040] Furthermore, the free radical initiator is one or more of azobisisobutyronitrile (AIBN) and benzoyl peroxide (BPO).

[0041] Preferably, the free radical initiator is azobisisobutyronitrile (AIBN), which accounts for 0.5% by mass in the composite liquid electrolyte.

[0042] Furthermore, the conductive agent is one or more of acetylene black, carbon nanotubes, graphite, and graphene.

[0043] Preferably, the conductive agent is carbon nanotubes, which account for 12% by mass in the high-load positive electrode.

[0044] Furthermore, the nanoscale positive electrode material is lithium iron phosphate (LiFePO4), lithium nickel cobalt manganese oxide (LiNi 1-x- y Mnx Co y O2), lithium cobalt oxide (LiCoO2), lithium manganese oxide (LiMn2O4), lithium-rich manganese-based (Li 1+x MnO2) or more.

[0045] Preferably, the nanoscale positive electrode material is lithium iron phosphate (LiFePO4), which accounts for 75% by mass in the high-load positive electrode.

[0046] Furthermore, the stirring time before obtaining the precursor solution is 0.5-12h.

[0047] Preferably, the stirring time before obtaining the precursor solution is 1 hour.

[0048] Furthermore, the mixing and stirring time before obtaining the composite liquid electrolyte is 0.5-12h.

[0049] Preferably, the time of blending and stirring before obtaining the composite liquid electrolyte is 4 hours.

[0050] Furthermore, the temperature of high-temperature thermal polymerization of the composite solid electrolyte is 40-100° C., and the thermal polymerization time is 0.5-24 h.

[0051] Preferably, the temperature of high-temperature thermal polymerization to obtain the composite solid electrolyte is 80° C., and the thermal polymerization time is 12 hours.

[0052] Furthermore, in the method for preparing the high-load positive electrode, the grinding and blending time is 1-8 hours; the thermal polymerization temperature is 40-80° C., and the time is 0.5-24 hours.

[0053] Preferably, in the method for preparing the high-load positive electrode, the grinding and blending time is 2 hours, the thermal polymerization temperature is 60° C., and the time is 1 hour.

[0054] Furthermore, the heating temperature of the integrated "electrode / electrolyte" is 30-50°C, the heating time is 10-60min, the high temperature standing temperature is 40-100°C, and the standing time is 1-24h.

[0055] Preferably, the heating temperature of the integrated "electrode / electrolyte" is 45°C, the heating time is 30 minutes, the high temperature standing temperature is 80°C, and the standing time is 12 hours.

[0056] In general, compared with the prior art, the above technical solutions conceived by the present invention provide a method for preparing an in-situ polymerized solid electrolyte, a solid electrolyte, an integrated "electrode / electrolyte" and a solid-state battery:

[0057] The solid electrolyte prepared by in-situ polymerization has high conductivity, high migration number and good electrode contact ability at room temperature, which is conducive to the construction of an enhanced electrode / electrolyte interface and effectively inhibits interfacial side reactions, so that the assembled solid-state lithium metal battery exhibits high surface capacity and ultra-long cycle life at room temperature. Specifically, the ionic conductivity of the optimized composite solid electrolyte can reach 0.37mS / cm. At the same time, the assembled low-load lithium iron phosphate solid-state battery has a capacity retention rate of more than 95% after 250 cycles at a 1C rate; the assembled high-load lithium iron phosphate solid-state battery has a performance of up to 1.6mAh / cm 2 The high surface capacity and high specific capacity of 159 mAh / g.

[0058] The present invention has the following beneficial effects:

[0059] (1) In the preparation method provided by the present invention, compared with the traditional solvent method for preparing solid electrolytes alone, the solid-state battery prepared by the in-situ polymerization method not only utilizes the high permeability of the electrolyte before polymerization, solves the interface problem and ion conduction problem between the electrolyte and the electrode, but also abandons the complex processes such as dissolution and drying film formation caused by the solvent method, effectively improves the utilization rate of raw materials, is environmentally friendly, and reduces costs.

[0060] (2) In the preparation method of the present invention, compared with the conventional in-situ polymerization method using glass fiber or diaphragm ion-conducting inert materials as the self-supporting structure, the in-situ polymerization technology used in the present invention uses active fillers as the self-supporting structure to construct a variety of ion conduction channels, thereby better ensuring the ion transport inside the electrolyte.

[0061] (3) In the preparation method of the present invention, the high-load positive electrode prepared by the present invention does not need to be dried, thereby avoiding electrode cracking, while the polymer used as the binder in the traditional positive electrode preparation is prone to electrode cracking during the high-temperature drying process.

[0062] (4) In the preparation method of the present invention, the high-load electrode prepared by the conventional wet method has poor conductivity during the charge and discharge process, and the capacity of the active material is difficult to fully utilize. The present invention increases the internal ion transmission channel of the electrode through in-situ polymerization, and fully utilizes the active material inside the electrode. BRIEF DESCRIPTION OF THE DRAWINGS

[0063] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0064] Figure 1Graphs showing ionic conductivity of composite solid electrolytes of different lithium salts prepared in Example 1, Example 2 and Example 3 at different temperatures.

[0065] Figure 2 Graphs showing the electronic conductivity of composite solid electrolytes of different lithium salts prepared in Example 1, Example 2 and Example 3 at room temperature.

[0066] Figure 3 The polarization voltage diagrams of the composite solid electrolyte 1 prepared in Example 1, Example 2 and Example 3 after assembling a lithium symmetric battery at room temperature and conducting tests at different current densities are shown.

[0067] Figure 4 The lithium iron phosphate prepared in Example 4 (conventional method and in-situ polymerization method) and Example 5 has a loading of about 1.5 mg / cm 2 Long cycle performance diagram of the assembled low-load solid-state battery at a current density of 1C (1C = 170 mAh / g).

[0068] Figure 5 The integrated battery assembled with high-load "electrode / electrolyte" prepared in Example 4 and Example 5 was 0.1 mA / cm 2 Cycling performance diagram at different current densities. DETAILED DESCRIPTION

[0069] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0070] Example 1: Preparation of precursor solution

[0071] (1) In a glove box where the water and oxygen concentrations are less than 0.1 ppm, 0.005 mol of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) was weighed and dissolved in a mixed solution of 1 mL of trifluoroethyl methacrylate (TFEMA), 3.95 mL of fluoroethylene carbonate (FEC), and 0.05 mL of pentaerythritol tetraacrylate (PETA), and stirred for 1 h to obtain a uniformly mixed precursor solution 1.

[0072] (2) In a glove box where the water and oxygen concentrations are both less than 0.1 ppm, 1.0135 g of a combined salt of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and 0.1014 g of lithium nitrate (LiNO3) were weighed and dissolved in a mixed solution of 1 mL of trifluoroethyl methacrylate (TFEMA), 3.95 mL of fluoroethylene carbonate (FEC), and 0.05 mL of pentaerythritol tetraacrylate (PETA), and stirred for 1 h to obtain a uniformly mixed precursor solution 2.

[0073] Example 2: Preparation of composite solid electrolyte

[0074] (1) In a glove box where the water and oxygen concentrations are less than 0.1 ppm, 1 g of nano-lithium iron phosphate, 4 g of the precursor solution 1 described in Example 1, and 0.0040 g of azobisisobutyronitrile were weighed and stirred at room temperature for 4 h to obtain a uniformly mixed composite liquid electrolyte 1.

[0075] (2) In a glove box where the water and oxygen concentrations are less than 0.1 ppm, 1 g of nano-lithium iron phosphate, 4 g of the precursor solution 2 described in Example 1, and 0.0040 g of azobisisobutyronitrile were weighed and stirred at room temperature for 4 h to obtain a uniformly mixed composite liquid electrolyte 2.

[0076] Example 3: Preparation of a symmetrical battery containing a composite solid electrolyte

[0077] (1) The composite liquid electrolyte 1 and the composite liquid electrolyte 2 described in Example 2 were respectively assembled in a stainless steel symmetrical battery, packaged, and thermally polymerized at 80° C. for 12 h to obtain a stainless steel symmetrical battery containing the composite solid electrolyte 1 and the composite solid electrolyte 2, respectively, which was used for impedance test of electrical conductivity and electronic resistance test. After the test, the battery was disassembled for electrolyte thickness test.

[0078] (2) The composite liquid electrolyte 1 described in Example 2 was assembled into lithium metal symmetrical batteries, packaged, and thermally polymerized at 80° C. for 12 h to obtain lithium symmetrical batteries containing the composite solid electrolyte 1, which were used to detect their stability to lithium.

[0079] Figure 1 The ionic conductivity curves of different composite solid electrolytes at different temperatures. Obviously, the solid electrolytes prepared by different lithium salts are all higher than 0.32mS / cm at room temperature, which is attributed to the formation of multiphase ion transport channels, giving full play to the transport paths of ions in the organic phase, inorganic phase and organic-inorganic phase interface, further illustrating that the composite solid electrolyte prepared by the in-situ polymerization method is capable of operating at room temperature. Figure 2The electronic conductivity bar graph of different composite solid electrolytes at room temperature is shown in Figure 1. Obviously, the electronic conductivity is 6 orders of magnitude lower than the ionic conductivity test value, which ensures that the composite solid electrolyte prepared by the in-situ polymerization method has a lower electronic conductivity, which is beneficial to prevent self-discharge behavior. Figure 3 Polarization voltage curves of lithium symmetric batteries assembled with the composite solid electrolyte 1 at different current densities at room temperature show that the composite solid electrolyte 1 has extremely strong stability to lithium and can withstand 1.5 mA / cm 2 The current density provides feasibility for the development of high surface capacity batteries.

[0080] Example 4: Preparation of electrodes

[0081] (1) In a glove box where the water and oxygen concentrations are less than 0.1 ppm, dissolve 0.0010 g of azobisisobutyronitrile in 1 g of precursor solution 1 to obtain a mixed solution. Weigh 0.1200 g of carbon nanotubes and 0.7500 g of lithium iron phosphate powder in a dry mortar and grind for 1 hour, drop 0.1300 g of the mixed solution, and continue grinding for 2 hours to obtain an active slurry. Then, coat the active slurry on aluminum foil, place it on a 60°C heating plate and heat it for 1 hour to obtain a positive electrode prepared by in situ polymerization. Among them, the active material (lithium iron phosphate) loading is less than 3 mg / cm 2 The electrode is a low-load electrode, higher than 10 mg / cm 2 High-capacity electrode.

[0082] (2) Conventional positive electrode preparation: 0.2000g lithium iron phosphate powder, 0.0250g acetylene black powder and 0.0250g polyvinylidene fluoride powder (PVDF) were weighed and ground in a mortar for 30 minutes, transferred to a weighing bottle, and then 8mL N-methylpyrrolidone (NMP) was added and stirred at room temperature for 5 hours to obtain a uniform mixed slurry. Then, the uniform mixed slurry was coated on aluminum foil and placed in a vacuum drying oven at 80°C for 12 hours to obtain a conventional wet-process prepared positive electrode.

[0083] Example 5: Preparation of integrated “electrode / electrolyte”

[0084] The composite liquid electrolyte 1 prepared in Example 1 was applied to the positive electrode prepared in Example 4, and heated on a 45°C heating plate for 30 minutes, and then placed in a 2025 button battery, and a lithium sheet was stacked on the electrolyte side, and packaged to obtain a solid-state battery. The solid-state battery was placed in an 80°C blast oven for 12 hours and then subjected to electrochemical testing.

[0085] The solid-state battery was placed in a Neware battery test system for electrochemical performance testing, using a constant current charge / discharge method: the charge and discharge voltage window was set to 2.7-4.0V, and the theoretical specific capacity was 170mAh / g.

[0086] Figure 4 The loading capacity of the conventional method and the in-situ polymerization method is about 1.5 mg / cm 2 The long cycle performance diagram of the low-load integrated "electrode / electrolyte" solid-state battery assembled with lithium iron phosphate at a current density of 1C (1C = 170mAh / g). As can be seen from the figure, the low-load integrated battery constructed by the in-situ polymerization method has excellent cycle stability and shows a similar performance trend to the conventional positive electrode, but has a discharge specific capacity that is superior to the conventional positive electrode, up to 145mAh / g, which further illustrates that the positive electrode prepared by the in-situ polymerization method has better ion transport capabilities than the conventional method. In addition, the surface capacity of the low-load integrated battery obtained by the in-situ polymerization method is about 0.162mA / cm 2 , and after 250 cycles, the capacity retention rate can still be more than 95%. Figure 5 The high-load "electrode / electrolyte" integrated solid-state battery constructed by the in-situ polymerization method is 0.1 mA / cm 2 Cyclic performance diagram at a current density of 1.38 Å, with a lithium iron phosphate loading of up to 11 mg / cm2 in the electrode. 2 During the cycle, the specific capacity can reach 159 mAh / g and the surface capacity can reach 1.6 mAh / cm 2 Compared with low-load lithium iron phosphate batteries (-1.5mg / cm 2 ), the surface capacity increased by nearly 10 times, further proving the feasibility of preparing integrated "electrode / electrolyte" by in situ polymerization.

[0087] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a high surface capacity lithium metal solid-state battery, characterized in that: include: S1. The lithium salt, polymer monomer, thickener and crosslinking agent are stirred and mixed to obtain a uniform precursor solution; S2. The precursor solution is blended and stirred with a nanoscale active filler and a free radical initiator to obtain a thick composite liquid electrolyte, and the composite liquid electrolyte is subjected to thermal polymerization to obtain a composite solid electrolyte; S3. Adding a conductive agent, a nanoscale cathode material and a free radical initiator to the precursor solution, stirring and blending, pouring the mixture into an aluminum foil, and thermally polymerizing to obtain a cathode; S4. dripping a composite liquid electrolyte onto the positive electrode, heating it, assembling a battery with a lithium negative electrode, heating and allowing it to stand, to obtain a high surface capacity lithium metal solid-state battery.

2. The preparation method according to claim 1, characterized in that: The lithium salt concentration is 0.2-1.5 mol / L; the volume fraction of the polymer monomer is 4-30 vol%; the volume fraction of the thickener is 60-95 vol%; the volume fraction of the cross-linking agent is 1-10 vol%; the mass fraction of the nanoscale active filler is 5-60%; the mass fraction of the free radical initiator is 0.2-5%; the mass fraction of the precursor solution in the high-load positive electrode is 2-10%; the mass fraction of the conductive agent is 2-10%; the mass fraction of the nanoscale positive electrode material is 70-95%.

3. The preparation method according to claim 1, characterized in that: The lithium salt is one or more of lithium bis(trifluoromethanesulfonyl imide), lithium bis(fluorosulfonyl imide), lithium hexafluorophosphate, lithium tetrafluoroborate, lithium nitrate, lithium difluorooxalatoborate, and lithium difluorophosphate; the polymer monomer is one or more of butyl acrylate, polyethylene glycol diacrylate, ethyl cyanoacrylate, and trifluoroethyl methacrylate; the thickener is one or more of ethylene carbonate, fluoroethylene carbonate, vinylene carbonate, and succinonitrile; the crosslinking agent is one or more of methacrylate, pentaerythritol tetraacrylate, propylene glycol acrylate, and glycerol acrylate.

4. The preparation method according to claim 1, characterized in that: The nano active filler is garnet-type Li 3+ x A3B2O 12 One or more of oxides, sulfides, lithium iron phosphate, lithium nickel cobalt manganese oxide, and lithium cobalt oxide; the free radical initiator is one or more of azobisisobutyronitrile and benzoyl peroxide.

5. The preparation method according to claim 1, characterized in that: The conductive agent is one or more of acetylene black, carbon nanotubes, graphite, and graphene; the nanoscale positive electrode material is one or more of lithium iron phosphate, lithium nickel cobalt manganese oxide, lithium cobalt oxide, lithium manganese oxide, and lithium-rich manganese base.

6. The preparation method according to claim 1, characterized in that: The stirring time before obtaining the precursor solution in step S1 is 0.5-12h.

7. The preparation method according to claim 1, characterized in that: The time of mixing and stirring before obtaining the composite liquid electrolyte in step S2 is 0.5-12 hours; the temperature of high-temperature thermal polymerization to obtain the composite solid electrolyte is 40-100° C., and the thermal polymerization time is 0.5-24 hours.

8. The preparation method according to claim 1, characterized in that: The grinding and blending time in the preparation method of the high-load positive electrode in step S3 is 1-8 hours; the thermal polymerization temperature is 40-80° C., and the time is 0.5-24 hours.

9. The preparation method according to claim 1, characterized in that: In step S4, the heating temperature is 30-50°C, the heating time is 10-60 minutes, the heating standing temperature is 40-100°C, and the standing time is 1-24 hours.

10. A high surface capacity lithium metal solid-state battery prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Solid electrolyte as well as preparation method and application thereof

    CN110048156A

  • Composite solid electrolyte positive electrode piece as well as preparation method and application thereof

    CN110176576A

  • Preparation method of in-situ thermal polymerization solid-state lithium-sulfur battery

    CN115241541A

  • Preparation method of high-voltage lithium metal battery based on in-situ curing

    CN115911581A

Cited By

  • Composite solid electrolyte, preparation method thereof and secondary battery containing composite solid electrolyte

    CN122091709A