Preparation method of ceramic core for controlling recrystallization of inner cavity of single-crystal hollow blade

By using the press-in molding method of cold core mold and ceramic core mold in the preparation of single crystal hollow blades, combining the mortise and tenon splicing structure and hot melt core, the ceramic core is solved by re-crystallization after high-temperature casting. and the problem of dimensional stability improves the casting pass rate and the bending strength of the ceramic core.

CN119057013AActive Publication Date: 2024-12-03AVIC BEIJING INST OF AERONAUTICAL MATERIALS

Patent Information

Application Number
CN202411562453.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-05
Publication Date
2024-12-03
Estimated Expiration
2044-11-05

AI Technical Summary

Technical Problem

The prior art is difficult to effectively control the recrystallization problem of the inner cavity of single crystal hollow blades by hot pressing molding, and the ceramic core is prone to dimensional shrinkage and surface cracks after high-temperature casting.

Method used

The compression molding method of cold core molds and ceramic core molds is carried out successively. Through the combination of mortise and tenon splicing structure and hot melt core slurry, the thickness ratio and material ratio of the ceramic core are adjusted to ensure that the ceramic core is in The hot melt core is removed during the firing process, which reduces cracks caused by thermal expansion mismatch, and improves the bending strength of the ceramic core.

Benefits of technology

The ceramic core is realized to maintain dimensional accuracy and performance after high-temperature casting, effectively control the recrystallization of the cavity of single crystal hollow blades, improve the casting pass rate, and solve the dimensional stability and rough surface of the ceramic core with a thickness larger than that of ceramic core. degree problem.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119057013A_ABST
    Figure CN119057013A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a ceramic core for controlling recrystallization of an inner cavity of a single-crystal hollow blade, which comprises the following steps: injecting ceramic core slurry into a cold core mold for primary mold filling and pressing to obtain an integrated cold core; part of the cold core is cut off from the integrated cold core, and the reserved part of the cold core is placed in the position, corresponding to the structure of the cold core, in the cold core mold; injecting the hot melting core slurry into a cold core mold for secondary mold filling pressing to obtain a mortise and tenon joint splicing type cold core; putting the mortise and tenon joint type cold core into a ceramic core mold, and injecting the ceramic core slurry into the ceramic core mold for mold filling and pressing to obtain a ceramic core green body; and roasting the ceramic core green body to obtain the ceramic core for controlling recrystallization of the inner cavity of the single crystal hollow blade. The prepared ceramic core has enough strength and good deformability, and the problem that recrystallization is likely to be generated in an inner cavity of the single crystal hollow blade after high-temperature pouring is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ceramic core preparation in single crystal hollow blade precision casting, and in particular relates to a ceramic core preparation method for controlling recrystallization of an inner cavity of a single crystal hollow blade. Background Art

[0002] At present, with the increase of the front inlet temperature of aircraft engines, higher requirements are put forward for the cooling effect of the inner cavity of hollow turbine blades. As an important adapter for forming the inner cavity of hollow turbine blades, the structure of ceramic cores is gradually developing towards large size, complexity and refinement with the increase of the demand for blade cooling effect. In particular, while the overall size of the ceramic core is thick and large, there will be small and fine flow-limiting structures in the local area, which leads to the thickness ratio of the ceramic core reaching more than 10, that is, the thickness of the thickest part of the ceramic core: the thickness of the thinnest part ≥ 10:1, and the existence of spoiler columns, impact holes and other structures in the thinner parts of the ceramic core makes the ceramic core have the following two prominent problems: First, it is difficult to complete the complete filling of the ceramic core through one-time hot pressing and injection molding, and the thin-walled part is prone to insufficient filling and resulting in virtual connection; second, the ceramic core at the thick-walled part is prone to shrinkage and deformation.

[0003] At the same time, the ceramic core used to prepare single-crystal hollow blades needs to have good yield properties to avoid recrystallization in the inner cavity of the blade. However, in the actual scientific research and production process, it is found that the location where the thickness of the blade cavity suddenly changes is prone to fine structures such as spoiler columns and impact holes, which leads to stress concentration and causes local recrystallization in the blade cavity. This problem has become a bottleneck in the development of my country's aero-engines and seriously restricts the production quality of single-crystal hollow blades. Therefore, it is urgent to develop a ceramic core preparation method for controlling the recrystallization of the inner cavity of single-crystal hollow blades, which can meet the quality requirements of the ceramic core (such as complete filling of the thin-walled position without virtual connection, and no dimensional shrinkage and deformation at the thick-walled position) while avoiding recrystallization of the inner cavity of the blade after casting.

[0004] The invention patent with application publication number CN117358887A discloses a control method for preparing the recrystallization of the inner cavity of a single crystal blade based on a photocuring ceramic core, including the following steps: the blade starts from the spiral of the crystal selector, and the blade proceeds from bottom to top along the solidification direction R; the blade wall is connected to the inner cavity partition, and recrystallization occurs on the inner cavity partition. The lower core and the upper core of the recrystallization are both provided with a local hollow structure, the hollow structure area of ​​the lower core is larger than the recrystallization size, and the hollow structure area of ​​the upper core is larger than half of the recrystallization size; the core is prepared by photocuring ceramic 3D printing technology. This technical solution adopts the photocuring 3D printing method to prepare the ceramic core, designs a local hollow structure, and increases the yield of the core. Although it can realize the control of the recrystallization of the inner cavity of the single crystal blade, the ceramic core prepared by the photocuring 3D printing method has relatively poor properties such as roughness and strength. At present, the hot pressing method is still used to prepare ceramic cores, because their shrinkage is more compatible with the subsequent ceramic shell, and the roughness, strength and other properties are better. Therefore, in order to control the recrystallization of the inner cavity of the single crystal hollow blade, it is necessary to explore a method for preparing ceramic cores suitable for hot pressing molding. The invention patent with application publication number CN114544631A discloses a method for evaluating the tendency of recrystallization formation of spoiler columns of single crystal high-temperature alloy hollow blades, including the following steps: pressing a ceramic core; pressing a wax mold and combining it into a module; coating the module with refractory materials, drying and sintering to obtain a shell mold (multi-layer structure), and then dewaxing and sintering; pouring different single crystal high-temperature alloys to prepare single crystal high-temperature alloy castings, and then performing shelling and core removal after cutting; vacuum heat treatment of single crystal high-temperature alloy castings, and then dissecting the castings along the height direction of the spoiler column, and macroscopic corrosion and inspection of recrystallization. This technical solution provides an evaluation method for recrystallization of the inner cavity of a single-crystal hollow blade with a spoiler column structure. It is found that the greater the number of recrystallizations, the larger the diameter of the spoiler column where the recrystallization occurs, and the larger the fillet radius, the greater the tendency of the spoiler column to recrystallize. This technical solution only provides an evaluation method for recrystallization of the inner cavity of the blade, and does not record how to avoid or control the recrystallization of the inner cavity of the blade. Summary of the invention

[0005] In order to solve the problems existing in the prior art, the present invention provides a method for preparing a ceramic core for controlling the recrystallization of the inner cavity of a single-crystal hollow blade. The preparation method comprises the following steps in chronological order: Step 1: Make a cold core mold according to the designed cold core structure, and use an injection molding machine to inject the ceramic core slurry into the cold core mold for one-time filling and pressing to obtain an integrated cold core; Step 2: Use a cutting tool to cut off part of the cold core from the integrated cold core, and cut the cut section of the integrated cold core into a mortise and tenon joint shape; Step 3: Place the remaining cold core on the integrated cold core into the cold core mold at a position corresponding to its structure, and use an injection molding machine to inject hot-melt core slurry into the cold core mold for secondary filling and pressing to obtain a mortise and tenon joint cold core; Step 4: manufacturing a ceramic core mold according to the designed ceramic core structure, placing the mortise and tenon joint cold core into the ceramic core mold, and injecting the ceramic core slurry into the ceramic core mold by an injection molding machine for filling and pressing to obtain a ceramic core blank; Step 5: Check the ceramic core blank and confirm that there are no obvious defects in its appearance, then insert the ceramic core blank into a calcined pot filled with kaolin filler, and make the kaolin filler completely cover the ceramic core blank; Step 6: Place the calcined pot containing the kaolin filler and the ceramic core blank into a calcining furnace for calcining. After the calcining is completed, a ceramic core for controlling the recrystallization of the inner cavity of the single crystal hollow blade is obtained.

[0006] Preferably, in step one, the pressing material of the integrated cold core is a ceramic core slurry, and the mass percentage of each substance in the ceramic core slurry is 70-85wt% of ceramic powder and 15-30wt% of plasticizer; the mass percentage of each substance in the ceramic powder is 70-90wt% of quartz glass powder, 5-20wt% of zirconium silicate powder, and 5-10wt% of mullite whisker, and the median particle size of the quartz glass powder and the zirconium silicate powder is 25-50μm; the mass percentage of each substance in the plasticizer is 80-85wt% of paraffin, 10-15wt% of beeswax, and 5-8wt% of polyethylene glycol.

[0007] The preparation process of the ceramic core slurry is as follows: first, quartz glass powder, zirconium silicate powder and mullite whisker are uniformly mixed at room temperature according to the designed material ratio to obtain ceramic powder; then, paraffin, beeswax and polyethylene glycol are placed in a container and heated to melt according to the designed material ratio, the heating temperature is 90-120° C., and the three substances are uniformly mixed to obtain a plasticizer; finally, the heating temperature is kept unchanged, the ceramic powder is added to the plasticizer and mixed uniformly to obtain the ceramic core slurry, and then the temperature is reduced to 80-100° C. and kept warm for standby use.

[0008] In any of the above schemes, preferably, in step 1, the pressing parameters of the integrated cold core are: injection temperature 80-100° C., injection pressure 3-5 MPa, and holding time 5-35 s.

[0009] In any of the above schemes, preferably, in step 2, cutting is performed according to the shape of the mortise and tenon connection, and the cut-off portion of the cold core is 33-50% of the integrated cold core.

[0010] In any of the above schemes, it is preferred that in step three, the mortise and tenon jointed cold core is formed by splicing a ceramic core slurry cold core and a hot melt core slurry cold core in a mortise and tenon manner; the ceramic core slurry cold core is pressed by ceramic core slurry, that is, a portion of the cold core retained from the integrated cold core; the hot melt core slurry cold core is pressed by hot melt core slurry, and its structure is the same as that of the portion of the cold core cut off from the integrated cold core.

[0011] In any of the above schemes, preferably, in step three, the mass percentage of each substance in the hot melt core slurry is 50-65wt% of polyethylene glycol, 30-40wt% of graphite powder, and 5-10wt% of stearic acid; the molecular weight of the polyethylene glycol is 2000-6000, and the particle size of the graphite powder is 325-800 mesh.

[0012] The preparation process of the hot-melt core slurry is as follows: firstly, each material is weighed according to the designed material ratio for use; then, polyethylene glycol and stearic acid are placed in a container and heated to melt, the heating temperature is 100-120° C., and the two materials are mixed evenly; finally, the heating temperature is kept unchanged, graphite powder is added into the container and mixed evenly with polyethylene glycol and stearic acid to obtain the hot-melt core slurry, and then the temperature is reduced to 65-80° C. and kept warm for use.

[0013] In any of the above schemes, it is preferred that in step three, the pressing parameters of the mortise and tenon joint cold core are: injection temperature 65-80°C, injection pressure 1.5-3MPa, and holding time 3-25s; after the pressing is completed, the room temperature three-point bending strength of the hot-melt core slurry cold core is 10-15MPa, and it can maintain its shape under an injection pressure below 10MPa, and can be subsequently removed during the sintering process of the ceramic core blank.

[0014] In any of the above schemes, preferably, in step 4, the pressing material of the ceramic core blank is a ceramic core slurry, and the mass percentage of each substance in the ceramic core slurry is 70-85wt% of ceramic powder and 15-30wt% of plasticizer; the mass percentage of each substance in the ceramic powder is 70-90wt% of quartz glass powder, 5-20wt% of zirconium silicate powder, and 5-10wt% of mullite whisker, and the median particle size of the quartz glass powder and the zirconium silicate powder are both 25-50μm; the mass percentage of each substance in the plasticizer is 80-85wt% of paraffin, 10-15wt% of beeswax, and 5-8wt% of polyethylene glycol.

[0015] The preparation process of the ceramic core slurry is as follows: first, quartz glass powder, zirconium silicate powder and mullite whisker are uniformly mixed at room temperature according to the designed material ratio to obtain ceramic powder; then, paraffin, beeswax and polyethylene glycol are placed in a container and heated to melt according to the designed material ratio, the heating temperature is 90-120° C., and the three substances are uniformly mixed to obtain a plasticizer; finally, the heating temperature is kept unchanged, the ceramic powder is added to the plasticizer and mixed uniformly to obtain the ceramic core slurry, and then the temperature is reduced to 80-100° C. and kept warm for standby use.

[0016] In any of the above schemes, preferably, in step 4, the pressing parameters of the ceramic core blank are: injection temperature 80-100° C., injection pressure 4-6 MPa, and holding time 5-35 s.

[0017] In any of the above schemes, it is preferred that in step six, the roasting process of the ceramic core blank is: placing the calcining bowl containing kaolin filler and the ceramic core blank into a roasting furnace, heating the temperature from room temperature to 200°C at a heating rate of 1-3°C / min, and keeping it warm for 0.5-2h; continuing to heat the temperature from 200°C to 900°C at a heating rate of 3-5°C / min, and keeping it warm for 1-3h; continuing to heat the temperature from 900°C to 1100-1300°C at a heating rate of 8-10°C / min, keeping it warm for 2-6h, and then cooling to room temperature with the furnace.

[0018] In the present invention, the injection molding machine, roasting furnace, etc. used are all traditional equipment, and there are no special requirements for the equipment structure and model. The manufacturing process of the cold core mold and the ceramic core mold is a traditional process, and there are no special requirements for the process flow, process parameters, mold materials, manufacturing equipment, etc.; at the same time, the pressing process of the integrated cold core, the mortise and tenon joint cold core, and the ceramic core blank is also a traditional process, and there are no special requirements for the process flow, process parameters, pressing equipment, etc., and it is only necessary to ensure that the injection temperature, injection pressure, holding time and other key pressing parameters meet the requirements of the present invention. In addition, in the entire preparation process of the ceramic core, the structural design, material ratio, pressing parameters of the integrated cold core and the mortise and tenon joint cold core, as well as the material ratio, pressing parameters, roasting parameters, etc. of the ceramic core blank are very important, and each parameter needs to work synergistically to achieve the expected technical effect of the present invention.

[0019] In the present invention, the mortise and tenon joint cold core is located in a relatively thick portion inside the ceramic core blank / ceramic core, especially the hot melt core slurry cold core is located inside the ceramic core blank / ceramic core and corresponds to a portion where recrystallization is easily generated in the inner cavity of the single crystal hollow blade. During the firing process of the ceramic core blank, the hot melt core slurry cold core is gradually removed. The thickness ratio of the ceramic core refers to the ratio between the thickness at the thickest position and the thickness at the thinnest position in the ceramic core.

[0020] The ceramic core preparation method for controlling the recrystallization of the inner cavity of a single-crystal hollow blade of the present invention has the following beneficial effects: (1) The present invention uses a hot injection molding method to prepare a ceramic core. The prepared ceramic core has good yield properties while ensuring sufficient strength, thereby solving the problem of recrystallization of the inner cavity of the single crystal hollow blade after high-temperature pouring of the ceramic core. At the same time, it can ensure that the dimensional accuracy and performance of the ceramic core are not affected, thereby improving the casting qualification rate of the single crystal hollow blade.

[0021] (2) If the thickness difference of the ceramic core is large (the thickness is relatively large, usually not less than 10, that is, the thickness of the thickest part of the ceramic core: the thickness of the thinnest part ≥ 10:1), then the ceramic core is likely to cause recrystallization in the inner cavity of the single crystal hollow blade after high-temperature pouring. The present invention provides a theoretical basis for the structural design of ceramic cores with a thickness ratio of 10 or above, and has a simple preparation process, a short preparation cycle, and high efficiency, and can effectively control the recrystallization of the inner cavity of the blade after high-temperature pouring.

[0022] (3) The present invention regulates the matrix components of the hot-melt core slurry, adjusts the molecular weight of polyethylene glycol, and adds an appropriate amount of graphite powder, thereby improving the bending strength of the hot-melt core while ensuring the roughness of the mold surface, thereby solving the problem of cracks and bulging on the surface of the ceramic core after firing due to the mismatch in thermal expansion coefficients between the hot-melt core and the ceramic core. Compared with water-soluble core materials, the present invention can reduce the dissolution process and preparation cycle, and can prepare hot-melt core parts that meet the application requirements of ceramic cores. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 A flow chart of a preferred embodiment of a method for preparing a ceramic core for controlling the recrystallization of the inner cavity of a single crystal hollow blade according to the present invention; Figure 2 for Figure 1 A schematic diagram of the structure of the integrated cold core in the embodiment shown; Figure 3 for Figure 1 A schematic diagram of the structure of the mortise and tenon joint type cold core in the embodiment shown; Figure 4 To adopt Figure 1 Partial photo of a single crystal hollow blade made of a ceramic core of the embodiment shown. The annotations in the figure are as follows: 1-integrated cold core, 2-mortise and tenon joint cold core, 201-ceramic core slurry cold core, 202-hot melt core slurry cold core, 203-mortise and tenon joint shape. DETAILED DESCRIPTION

[0024] In order to further understand the content of the present invention, the present invention will be described in detail below in conjunction with specific embodiments.

[0025] Embodiment 1: like Figure 1-3 As shown, according to a preferred embodiment of the method for preparing a ceramic core for controlling the recrystallization of the inner cavity of a single crystal hollow blade of the present invention, the preparation method comprises the following steps in chronological order: Step 1: a cold core mold is manufactured according to the designed cold core structure, and a ceramic core slurry is injected into the cold core mold by an injection molding machine for one-time filling and pressing to obtain an integrated cold core 1; Step 2: using a cutting tool to cut off a portion of the integrated cold core 1, and cutting the cut section of the integrated cold core 1 into a mortise and tenon joint shape 203; Step 3: Place the remaining cold core of the integrated cold core 1 into the cold core mold at a position corresponding to its structure, and use an injection molding machine to inject hot-melt core slurry into the cold core mold for secondary filling and pressing to obtain the mortise and tenon joint cold core 2; Step 4: making a ceramic core mold according to the designed ceramic core structure, and placing the mortise and tenon joint cold core 2 into the ceramic core mold, and injecting the ceramic core slurry into the ceramic core mold by an injection molding machine for filling and pressing to obtain a ceramic core blank; Step 5: Check the ceramic core blank and confirm that there are no obvious defects in its appearance, then insert the ceramic core blank into a calcined pot filled with kaolin filler, and make the kaolin filler completely cover the ceramic core blank; Step 6: Place the calcined pot containing the kaolin filler and the ceramic core blank into a calcining furnace for calcining. After the calcining is completed, a ceramic core for controlling the recrystallization of the inner cavity of the single crystal hollow blade is obtained.

[0026] In step one, the pressing material of the integrated cold core 1 is a ceramic core slurry, and the mass percentage of each substance in the ceramic core slurry is 78wt% of ceramic powder and 22wt% of plasticizer; the mass percentage of each substance in the ceramic powder is 80wt% of quartz glass powder, 12wt% of zirconium silicate powder, and 8wt% of mullite whisker, and the median particle size of the quartz glass powder and the zirconium silicate powder is 38μm; the mass percentage of each substance in the plasticizer is 82wt% of paraffin, 12wt% of beeswax, and 6wt% of polyethylene glycol.

[0027] The preparation process of the ceramic core slurry is as follows: first, quartz glass powder, zirconium silicate powder and mullite whisker are mixed uniformly at room temperature according to the designed material ratio to obtain ceramic powder; then, paraffin, beeswax and polyethylene glycol are placed in a container and heated to melt according to the designed material ratio, the heating temperature is 105° C., and the three substances are mixed uniformly to obtain a plasticizer; finally, the heating temperature is kept unchanged, the ceramic powder is added to the plasticizer and mixed uniformly to obtain the ceramic core slurry, and then the temperature is reduced to 90° C. and kept warm for standby use.

[0028] The pressing parameters of the integrated cold core 1 are: injection temperature 90° C., injection pressure 4 MPa, and holding time 20 s.

[0029] In step 2, cutting is performed according to the mortise and tenon joint shape 203 , and the cut-off portion of the cold core accounts for 42% of the integrated cold core 1 .

[0030] In step three, the mortise and tenon jointed cold core 2 is formed by joining a ceramic core slurry cold core 201 and a hot melt core slurry cold core 202 in a mortise and tenon manner; the ceramic core slurry cold core 201 is pressed by ceramic core slurry, that is, a portion of the cold core retained from the integrated cold core 1; the hot melt core slurry cold core 202 is pressed by hot melt core slurry, and its structure is the same as that of the portion of the cold core cut off from the integrated cold core 1.

[0031] The mass percentages of the substances in the hot melt core slurry are 58wt% polyethylene glycol, 35wt% graphite powder, and 7wt% stearic acid; the molecular weight of the polyethylene glycol is 4000, and the particle size of the graphite powder is 500 mesh.

[0032] The preparation process of the hot-melt core slurry is as follows: first, weigh each material according to the designed material ratio for use; then, put polyethylene glycol and stearic acid into a container and heat to melt, the heating temperature is 110° C., and the two materials are mixed evenly; finally, keep the heating temperature unchanged, add graphite powder into the container and mix it evenly with polyethylene glycol and stearic acid to obtain the hot-melt core slurry, and then cool it to 72° C. and keep it warm for use.

[0033] The pressing parameters of the mortise and tenon joint cold core 2 are: injection temperature 72°C, injection pressure 2.2MPa, and holding time 14s; after the pressing is completed, the room temperature three-point bending strength of the hot-melt core slurry cold core is 12MPa, and it can maintain its shape under an injection pressure below 10MPa, and can be removed later during the ceramic core blank roasting process.

[0034] In step 4, the pressing material of the ceramic core blank is a ceramic core slurry, and the mass percentage of each substance in the ceramic core slurry is 78wt% of ceramic powder and 22wt% of plasticizer; the mass percentage of each substance in the ceramic powder is 80wt% of quartz glass powder, 12wt% of zirconium silicate powder, and 8wt% of mullite whisker, and the median particle size of the quartz glass powder and the zirconium silicate powder is 38μm; the mass percentage of each substance in the plasticizer is 82wt% of paraffin, 12wt% of beeswax, and 6wt% of polyethylene glycol.

[0035] The preparation process of the ceramic core slurry is as follows: first, quartz glass powder, zirconium silicate powder and mullite whisker are mixed uniformly at room temperature according to the designed material ratio to obtain ceramic powder; then, paraffin, beeswax and polyethylene glycol are placed in a container and heated to melt according to the designed material ratio, the heating temperature is 105° C., and the three substances are mixed uniformly to obtain a plasticizer; finally, the heating temperature is kept unchanged, the ceramic powder is added to the plasticizer and mixed uniformly to obtain the ceramic core slurry, and then the temperature is reduced to 90° C. and kept warm for standby use.

[0036] The pressing parameters of the ceramic core blank are: injection temperature 90° C., injection pressure 5 MPa, and holding time 20 s.

[0037] In step six, the calcination process of the ceramic core blank is as follows: place the calcination pot containing the kaolin filler and the ceramic core blank into a calcination furnace, and heat the temperature from room temperature to 200°C at a heating rate of 2°C / min, and keep it warm for 1.2 hours; continue to heat the temperature from 200°C to 900°C at a heating rate of 4°C / min, and keep it warm for 2 hours; continue to heat the temperature from 900°C to 1200°C at a heating rate of 9°C / min, and keep it warm for 4 hours, and then cool it to room temperature with the furnace. The ceramic core prepared in this embodiment is used to prepare a single crystal hollow blade. A partial photo of the single crystal hollow blade is shown in FIG. Figure 4 As shown in the figure, it can be seen that there is no recrystallization in the blade cavity.

[0038] In this embodiment, the injection molding machine, roasting furnace, etc. used are all traditional equipment, and there are no special requirements for the equipment structure and model. The manufacturing process of the cold core mold and the ceramic core mold is a traditional process, and there are no special requirements for the process flow, process parameters, mold materials, manufacturing equipment, etc.; at the same time, the pressing process of the integrated cold core, the mortise and tenon joint cold core, and the ceramic core blank is also a traditional process, and there are no special requirements for the process flow, process parameters, pressing equipment, etc., and it is only necessary to ensure that the injection temperature, injection pressure, holding time and other key pressing parameters meet the requirements of the present invention. In addition, in the entire preparation process of the ceramic core, the structural design, material ratio, pressing parameters of the integrated cold core and the mortise and tenon joint cold core, as well as the material ratio, pressing parameters, roasting parameters, etc. of the ceramic core blank are very important, and each parameter needs to work together to achieve the expected technical effect of this embodiment.

[0039] In this embodiment, the mortise and tenon joint cold core is located in a relatively thick portion inside the ceramic core blank / ceramic core, especially the hot melt core slurry cold core is located inside the ceramic core blank / ceramic core and corresponds to a portion where recrystallization is easily generated in the inner cavity of the single crystal hollow blade. During the firing process of the ceramic core blank, the hot melt core slurry cold core is gradually removed. The thickness ratio of the ceramic core refers to the ratio between the thickness at the thickest position and the thickness at the thinnest position in the ceramic core.

[0040] The present embodiment provides a method for preparing a ceramic core for controlling the recrystallization of the inner cavity of a single-crystal hollow blade, which has the following beneficial effects: (1) The ceramic core is prepared by hot injection molding, and the prepared ceramic core has good yielding property while ensuring sufficient strength, which solves the problem that the ceramic core causes the inner cavity of the single-crystal hollow blade to recrystallize after high-temperature pouring, and at the same time ensures that the dimensional accuracy and performance of the ceramic core are not affected, thereby improving the casting qualification rate of the single-crystal hollow blade. (2) A theoretical basis is provided for the structural design of a ceramic core with a thickness ratio of 10 or more, and the preparation process is simple, the preparation cycle is short, and the efficiency is high, which can effectively control the recrystallization of the inner cavity of the blade after high-temperature pouring. (3) By regulating the matrix component of the hot-melt core slurry, adjusting the molecular weight of polyethylene glycol, and adding an appropriate amount of graphite powder, the bending strength of the hot-melt core is improved while ensuring the roughness of the mold surface, which solves the problem that cracks and bulges appear on the surface of the ceramic core after sintering due to the mismatch between the thermal expansion coefficients of the hot-melt core and the ceramic core.

[0041] Embodiment 2: According to another preferred embodiment of the method for preparing a ceramic core for controlling the recrystallization of the inner cavity of a single crystal hollow blade of the present invention, the process flow, technical principle, beneficial effects, etc. are basically the same as those of the first embodiment, except that: In step one, the pressing material of the integrated cold core is a ceramic core slurry, and the mass percentage of each substance in the ceramic core slurry is 70wt% of ceramic powder and 30wt% of plasticizer; the mass percentage of each substance in the ceramic powder is 70wt% of quartz glass powder, 20wt% of zirconium silicate powder, and 10wt% of mullite whisker, and the median particle size of the quartz glass powder and the zirconium silicate powder is 25μm; the mass percentage of each substance in the plasticizer is 80wt% of paraffin, 15wt% of beeswax, and 5wt% of polyethylene glycol.

[0042] The preparation process of the ceramic core slurry is as follows: first, quartz glass powder, zirconium silicate powder and mullite whisker are mixed evenly at room temperature according to the designed material ratio to obtain ceramic powder; then, paraffin wax, beeswax and polyethylene glycol are placed in a container and heated to melt according to the designed material ratio, the heating temperature is 90°C, and the three substances are mixed evenly to obtain a plasticizer; finally, the heating temperature is kept unchanged, the ceramic powder is added to the plasticizer and mixed evenly to obtain a ceramic core slurry, and then the temperature is reduced to 80°C and kept warm for use. The pressing parameters of the integrated cold core are: injection temperature 80°C, injection pressure 3MPa, and holding time 35s.

[0043] In step 2, cutting is performed according to the shape of the mortise and tenon joints, and the cut-off portion of the cold core is 33% of the integrated cold core.

[0044] In step three, the mortise and tenon joint cold core is formed by joining a ceramic core slurry cold core and a hot melt core slurry cold core in a mortise and tenon manner; the ceramic core slurry cold core is pressed from a ceramic core slurry, that is, a portion of the cold core retained from an integrated cold core; the hot melt core slurry cold core is pressed from a hot melt core slurry, and its structure is the same as the portion of the cold core cut from an integrated cold core. The mass percentage of each substance in the hot melt core slurry is 50wt% polyethylene glycol, 40wt% graphite powder, and 10wt% stearic acid; the molecular weight of the polyethylene glycol is 2000, and the particle size of the graphite powder is 325 mesh.

[0045] The preparation process of the hot-melt core slurry is as follows: first, weigh each material according to the designed material ratio for use; then put polyethylene glycol and stearic acid into a container and heat to melt, the heating temperature is 100°C, and the two substances are mixed evenly; finally, keep the heating temperature unchanged, add graphite powder into the container and mix it evenly with polyethylene glycol and stearic acid to obtain hot-melt core slurry, then cool it to 65°C and keep it warm for use. The pressing parameters of the mortise and tenon joint cold core are: injection temperature 65°C, injection pressure 1.5MPa, and holding time 25s; after the pressing is completed, the room temperature three-point bending strength of the hot-melt core slurry cold core is 10MPa, and it can keep its shape unchanged under injection pressure below 10MPa, and can be removed later during the ceramic core blank roasting process.

[0046] In step 4, the pressing material of the ceramic core blank is a ceramic core slurry, and the mass percentage of each substance in the ceramic core slurry is 70wt% of ceramic powder and 30wt% of plasticizer; the mass percentage of each substance in the ceramic powder is 70wt% of quartz glass powder, 20wt% of zirconium silicate powder, and 10wt% of mullite whisker, and the median particle size of the quartz glass powder and the zirconium silicate powder is 25μm; the mass percentage of each substance in the plasticizer is 80wt% of paraffin, 15wt% of beeswax, and 5wt% of polyethylene glycol.

[0047] The preparation process of the ceramic core slurry is as follows: first, quartz glass powder, zirconium silicate powder, and mullite whisker are mixed uniformly at room temperature according to the designed material ratio to obtain ceramic powder; then, paraffin, beeswax, and polyethylene glycol are placed in a container and heated to melt according to the designed material ratio, the heating temperature is 90°C, and the three substances are mixed uniformly to obtain a plasticizer; finally, the heating temperature is kept unchanged, the ceramic powder is added to the plasticizer and mixed uniformly to obtain a ceramic core slurry, and then the temperature is reduced to 80°C and kept warm for use. The pressing parameters of the ceramic core blank are: injection temperature 80°C, injection pressure 4MPa, and holding time 35s.

[0048] In step 5, the ceramic core blank is inspected to confirm that there are no obvious defects in its appearance, and then the ceramic core blank is inserted into a calcined pot filled with kaolin filler, and the kaolin filler completely covers the ceramic core blank.

[0049] In step six, the roasting process of the ceramic core blank is as follows: place the calcining bowl containing kaolin filler and the ceramic core blank into a roasting furnace, heat the temperature from room temperature to 200°C at a heating rate of 1°C / min, and keep it warm for 2 hours; continue to heat the temperature from 200°C to 900°C at a heating rate of 3°C / min, and keep it warm for 3 hours; continue to heat the temperature from 900°C to 1100°C at a heating rate of 8°C / min, and keep it warm for 6 hours, and then cool to room temperature with the furnace.

[0050] Embodiment three: According to another preferred embodiment of the method for preparing a ceramic core for controlling the recrystallization of the inner cavity of a single crystal hollow blade of the present invention, the process flow, technical principle, beneficial effects, etc. are basically the same as those of the first embodiment, except that: In step one, the pressing material of the integrated cold core is a ceramic core slurry, and the mass percentage of each substance in the ceramic core slurry is 85wt% of ceramic powder and 15wt% of plasticizer; the mass percentage of each substance in the ceramic powder is 90wt% of quartz glass powder, 5wt% of zirconium silicate powder, and 5wt% of mullite whisker, and the median particle size of the quartz glass powder and the zirconium silicate powder is 50μm; the mass percentage of each substance in the plasticizer is 85wt% of paraffin, 10wt% of beeswax, and 5wt% of polyethylene glycol.

[0051] The preparation process of the ceramic core slurry is as follows: first, quartz glass powder, zirconium silicate powder and mullite whisker are mixed evenly at room temperature according to the designed material ratio to obtain ceramic powder; then, paraffin wax, beeswax and polyethylene glycol are placed in a container and heated to melt according to the designed material ratio, the heating temperature is 120°C, and the three substances are mixed evenly to obtain a plasticizer; finally, the heating temperature is kept unchanged, the ceramic powder is added to the plasticizer and mixed evenly to obtain a ceramic core slurry, and then the temperature is reduced to 100°C and kept warm for use. The pressing parameters of the integrated cold core are: injection temperature 100°C, injection pressure 5MPa, and holding time 5s.

[0052] In step 2, cutting is performed according to the shape of the mortise and tenon joints, and the cut-off portion of the cold core is 50% of the integrated cold core.

[0053] In step three, the mortise and tenon joint cold core is formed by joining a ceramic core slurry cold core and a hot melt core slurry cold core in a mortise and tenon manner; the ceramic core slurry cold core is pressed from a ceramic core slurry, that is, a portion of the cold core retained from an integrated cold core; the hot melt core slurry cold core is pressed from a hot melt core slurry, and its structure is the same as the portion of the cold core cut from an integrated cold core. The mass percentage of each substance in the hot melt core slurry is 65wt% polyethylene glycol, 30wt% graphite powder, and 5wt% stearic acid; the molecular weight of the polyethylene glycol is 6000, and the particle size of the graphite powder is 800 mesh.

[0054] The preparation process of the hot-melt core slurry is as follows: first, weigh each material according to the designed material ratio for use; then put polyethylene glycol and stearic acid into a container and heat to melt, the heating temperature is 120°C, and the two substances are mixed evenly; finally, keep the heating temperature unchanged, add graphite powder into the container and mix it evenly with polyethylene glycol and stearic acid to obtain hot-melt core slurry, then cool it to 80°C and keep it warm for use. The pressing parameters of the mortise and tenon joint cold core are: injection temperature 80°C, injection pressure 3MPa, and holding time 3s; after the pressing is completed, the room temperature three-point bending strength of the hot-melt core slurry cold core is 15MPa, and it can maintain its shape under an injection pressure below 10MPa, and can be removed later during the ceramic core blank roasting process.

[0055] In step 4, the pressing material of the ceramic core blank is a ceramic core slurry, and the mass percentage of each substance in the ceramic core slurry is 85wt% of ceramic powder and 15wt% of plasticizer; the mass percentage of each substance in the ceramic powder is 90wt% of quartz glass powder, 5wt% of zirconium silicate powder, and 5wt% of mullite whisker, and the median particle size of the quartz glass powder and the zirconium silicate powder is 50μm; the mass percentage of each substance in the plasticizer is 85wt% of paraffin, 10wt% of beeswax, and 5wt% of polyethylene glycol.

[0056] The preparation process of the ceramic core slurry is as follows: first, quartz glass powder, zirconium silicate powder, and mullite whisker are mixed uniformly at room temperature according to the designed material ratio to obtain ceramic powder; then, paraffin, beeswax, and polyethylene glycol are placed in a container and heated to melt according to the designed material ratio, the heating temperature is 120°C, and the three substances are mixed uniformly to obtain a plasticizer; finally, the heating temperature is kept unchanged, the ceramic powder is added to the plasticizer and mixed uniformly to obtain a ceramic core slurry, and then the temperature is reduced to 100°C and kept warm for standby use. The pressing parameters of the ceramic core blank are: injection temperature 100°C, injection pressure 6MPa, and holding time 5s.

[0057] In step 5, the ceramic core blank is inspected to confirm that there are no obvious defects in its appearance, and then the ceramic core blank is inserted into a calcined pot filled with kaolin filler, and the kaolin filler completely covers the ceramic core blank.

[0058] In step six, the roasting process of the ceramic core blank is as follows: place the calcination pot containing kaolin filler and the ceramic core blank into a roasting furnace, heat the temperature from room temperature to 200°C at a heating rate of 3°C / min, and keep it warm for 0.5h; continue to heat the temperature from 200°C to 900°C at a heating rate of 5°C / min, and keep it warm for 1h; continue to heat the temperature from 900°C to 1300°C at a heating rate of 10°C / min, and keep it warm for 2h, and then cool to room temperature with the furnace.

[0059] Special note: The technical solution of the present invention involves many parameters, and the synergistic effects between the various parameters need to be comprehensively considered to obtain the beneficial effects and significant progress of the present invention. Moreover, the value ranges of the various parameters in the technical solution are obtained after a large number of experiments. For each parameter and the combination of each parameter, the inventor has recorded a large amount of experimental data. Due to space limitations, the specific experimental data will not be disclosed here.

[0060] It is not difficult for those skilled in the art to understand that the ceramic core preparation method for controlling the recrystallization of the inner cavity of a single-crystal hollow blade of the present invention includes any combination of the invention content and specific implementation methods of the above-mentioned invention specification and the various parts shown in the drawings. Due to the limited space and to make the specification concise, the various schemes composed of these combinations are not described one by one. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a ceramic core for controlling the recrystallization of the inner cavity of a single-crystal hollow blade, Features: The preparation method comprises the following steps in chronological order: Step 1: Make a cold core mold according to the designed cold core structure, and use an injection molding machine to inject the ceramic core slurry into the cold core mold for one-time filling and pressing to obtain an integrated cold core; Step 2: Use a cutting tool to cut off part of the cold core from the integrated cold core, and cut the cut section of the integrated cold core into a mortise and tenon joint shape; Step 3: Place the remaining cold core on the integrated cold core into the cold core mold at a position corresponding to its structure, and use an injection molding machine to inject hot-melt core slurry into the cold core mold for secondary filling and pressing to obtain a mortise and tenon joint cold core; Step 4: manufacturing a ceramic core mold according to the designed ceramic core structure, placing the mortise and tenon joint cold core into the ceramic core mold, and injecting the ceramic core slurry into the ceramic core mold by an injection molding machine for filling and pressing to obtain a ceramic core blank; Step 5: Check the ceramic core blank and confirm that there are no obvious defects in its appearance, then insert the ceramic core blank into a calcined pot filled with kaolin filler, and make the kaolin filler completely cover the ceramic core blank; Step 6: Place the calcined pot containing the kaolin filler and the ceramic core blank into a calcining furnace for calcining. After the calcining is completed, a ceramic core for controlling the recrystallization of the inner cavity of the single crystal hollow blade is obtained.

2. The method for preparing a ceramic core for controlling the recrystallization of the inner cavity of a single crystal hollow blade according to claim 1, Features: In step 1, the pressing material of the integrated cold core is a ceramic core slurry, and the mass percentage of each substance in the ceramic core slurry is 70-85wt% of ceramic powder and 15-30wt% of plasticizer; the mass percentage of each substance in the ceramic powder is 70-90wt% of quartz glass powder, 5-20wt% of zirconium silicate powder, and 5-10wt% of mullite whisker, and the median particle size of the quartz glass powder and the zirconium silicate powder is 25-50μm; the mass percentage of each substance in the plasticizer is 80-85wt% of paraffin, 10-15wt% of beeswax, and 5-8wt% of polyethylene glycol; The preparation process of the ceramic core slurry is as follows: first, quartz glass powder, zirconium silicate powder and mullite whisker are uniformly mixed at room temperature according to the designed material ratio to obtain ceramic powder; then, paraffin, beeswax and polyethylene glycol are placed in a container and heated to melt according to the designed material ratio, the heating temperature is 90-120° C., and the three substances are uniformly mixed to obtain a plasticizer; finally, the heating temperature is kept unchanged, the ceramic powder is added to the plasticizer and mixed uniformly to obtain the ceramic core slurry, and then the temperature is reduced to 80-100° C. and kept warm for standby use.

3. The method for preparing a ceramic core for controlling the recrystallization of the inner cavity of a single crystal hollow blade according to claim 2, Features: In step 1, the pressing parameters of the integrated cold core are injection temperature 80-100° C., injection pressure 3-5 MPa, and holding time 5-35 s.

4. The method for preparing a ceramic core for controlling the recrystallization of the inner cavity of a single-crystal hollow blade according to claim 3, Features: In step 2, cutting is performed according to the shape of the mortise and tenon joints, and the cut-off portion of the cold core is 33-50% of the integrated cold core.

5. The method for preparing a ceramic core for controlling the recrystallization of the inner cavity of a single crystal hollow blade according to claim 4, Features: In step three, the mortise and tenon jointed cold core is formed by splicing a ceramic core slurry cold core and a hot melt core slurry cold core in a mortise and tenon manner; the ceramic core slurry cold core is pressed by ceramic core slurry, that is, the part of the cold core retained from the integrated cold core; the hot melt core slurry cold core is pressed by hot melt core slurry, and its structure is the same as the part of the cold core cut off from the integrated cold core.

6. The method for preparing a ceramic core for controlling the recrystallization of the inner cavity of a single-crystal hollow blade according to claim 5, Features: In step 3, the mass percentage of each substance in the hot melt core slurry is 50-65wt% of polyethylene glycol, 30-40wt% of graphite powder, and 5-10wt% of stearic acid; the molecular weight of the polyethylene glycol is 2000-6000, and the particle size of the graphite powder is 325-800 mesh; The preparation process of the hot-melt core slurry is as follows: first, weigh each material according to the designed material ratio for use; then put polyethylene glycol and stearic acid into a container and heat to melt, the heating temperature is 100-120° C., and the two materials are mixed evenly; finally, keep the heating temperature unchanged, add graphite powder into the container and mix it evenly with polyethylene glycol and stearic acid to obtain hot-melt core slurry, then cool it to 65-80° C., keep it warm for use.

7. The method for preparing a ceramic core for controlling the recrystallization of the inner cavity of a single crystal hollow blade according to claim 6, Features: In step three, the pressing parameters of the mortise and tenon joint cold core are injection temperature 65-80°C, injection pressure 1.5-3MPa, and holding time 3-25s; after the pressing is completed, the room temperature three-point bending strength of the hot-melt core slurry cold core is 10-15MPa, and it can maintain its shape under an injection pressure below 10MPa, and can be removed later during the sintering process of the ceramic core blank.

8. The method for preparing a ceramic core for controlling the recrystallization of the inner cavity of a single-crystal hollow blade according to claim 7, Features: In step 4, the pressing material of the ceramic core blank is a ceramic core slurry, and the mass percentage of each substance in the ceramic core slurry is 70-85wt% of ceramic powder and 15-30wt% of plasticizer; the mass percentage of each substance in the ceramic powder is 70-90wt% of quartz glass powder, 5-20wt% of zirconium silicate powder, and 5-10wt% of mullite whisker, and the median particle size of the quartz glass powder and the zirconium silicate powder is 25-50μm; the mass percentage of each substance in the plasticizer is 80-85wt% of paraffin, 10-15wt% of beeswax, and 5-8wt% of polyethylene glycol; The preparation process of the ceramic core slurry is as follows: first, quartz glass powder, zirconium silicate powder and mullite whisker are uniformly mixed at room temperature according to the designed material ratio to obtain ceramic powder; then, paraffin, beeswax and polyethylene glycol are placed in a container and heated to melt according to the designed material ratio, the heating temperature is 90-120° C., and the three substances are uniformly mixed to obtain a plasticizer; finally, the heating temperature is kept unchanged, the ceramic powder is added to the plasticizer and mixed uniformly to obtain the ceramic core slurry, and then the temperature is reduced to 80-100° C. and kept warm for standby use.

9. The method for preparing a ceramic core for controlling the recrystallization of the inner cavity of a single-crystal hollow blade according to claim 8, Features: In step 4, the pressing parameters of the ceramic core blank are injection temperature 80-100° C., injection pressure 4-6 MPa, and holding time 5-35 s.

10. The method for preparing a ceramic core for controlling the recrystallization of the inner cavity of a single crystal hollow blade according to claim 9, Features: In step six, the roasting process of the ceramic core blank is to place the calcination bowl containing kaolin filler and the ceramic core blank into a roasting furnace, and heat the temperature from room temperature to 200°C at a heating rate of 1-3°C / min, and keep it warm for 0.5-2h; continue to heat the temperature from 200°C to 900°C at a heating rate of 3-5°C / min, and keep it warm for 1-3h; continue to heat the temperature from 900°C to 1100-1300°C at a heating rate of 8-10°C / min, and keep it warm for 2-6h, and then cool it to room temperature with the furnace.

Citation Information

Patent Citations

  • Silicon oxide-based ceramic core for large-size directional hollow blade of heavy-duty gas turbine and preparation of silicon oxide-based ceramic core

    CN114249588A

  • Composite ceramic core for single crystal turbine blade and preparation method of composite ceramic core

    CN116477960A

  • Method for controlling recrystallization of inner cavity of single crystal blade prepared based on photocuring ceramic core

    CN117358887A

  • Double-wall cold ceramic core and hot-press injection integrated forming method

    CN118163209A

  • Ceramic core

    JP2022155407A

Cited By

  • High-deformability silicon-based ceramic core for nickel-based single crystal blade and preparation method of high-deformability silicon-based ceramic core