Preparation method and application of UV resin with UV and moist heat curing characteristics
Through the preparation method of solvent-free and catalyst-free UV resin, the problem of poor curing of UV materials in complex shapes or thick coatings is solved, and the UV resin with UV and moisture-heat curing characteristics is realized. It is suitable for battery insulating coatings of new energy vehicles and improves the improvement of UV and thermal insulation coatings. Productivity and environmental protection.
Patent Information
- Application Number
- CN202411321880.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-08-27
- Filing Date
- 2024-09-23
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing UV materials are prone to poor deep curing in opaque substrates, complex shapes or super-thick coatings, especially in formulations containing opaque mineral pigments, fillers or high-function powders, making it difficult to achieve uniform curing.
Using a solvent-free and catalyst-free UV resin preparation method, the polyurea reaction is activated by adding end-containing hydroxyacrylate monomer, polypropylene inhibitor and antioxidant to the reactor, vacuum dehydration and micro negative pressure control are carried out, and the polyurea reaction is activated to achieve UV resin synthesis with moisture and heat curing characteristics.
The prepared UV resin has low viscosity, transparent and clear, good adhesion and stability, and can be stored for a long time under cool and sealed conditions. It is suitable for various UV coatings, inks and glues, especially new energy vehicle battery insulating coatings. Improves curing speed and production efficiency, and reduces energy consumption and costs.
Smart Images

Figure CN119060299A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer material synthesis and application, and specifically relates to a method for preparing a UV resin with UV and wet heat curing properties and application thereof. Background Art
[0002] UV materials have 5E characteristics (environmental protection, high efficiency, energy saving, economy, functionality), no solvents, low halogen or halogen-free, lower viscosity, low organic emissions (VOC near zero), fast curing speed (calculated in seconds), good comprehensive performance of the cured film and many other advantages. They have now replaced solvent-based products and are widely used in coatings / inks / glue at home and abroad.
[0003] However, UV materials also have some defects: for example, between opaque substrates, coating areas with complex shapes that cannot be exposed to light or insufficient light, ultra-thick coatings (one-time curing exceeds 50 microns), opaque mineral pigment / filler formulas (especially white (reflects UV light, extinguishes free radicals), black (absorbs UV light, terminates and extinguishes free radicals), flame retardant, thermal conductive, insulating and other formulas with high mineral filler (absorbs UV light, terminates and extinguishes free radicals), and high-functional powder (absorbs UV light, terminates and extinguishes free radicals) content), deep curing is often poor, and the surface is dry but the inside is not dry.
[0004] Based on the above technical problems, it is still necessary to develop new UV resins and their supporting preparation methods. Summary of the invention
[0005] Purpose of the invention: The first purpose of the present invention is to provide a new preparation process for synthesizing a high-performance UV resin with UV and wet heat curing properties and the like, in view of the deficiencies in the prior art. The process does not require solvents and catalysts throughout the process, does not contain any ROHS banned substances, has a short reaction time, is easy to control the temperature during the synthesis process, has a mild reaction, and has no risks of temperature surge, gelation, sudden polymerization, and curing. The process is safe, environmentally friendly, stable, controllable, energy-saving, and efficient. The product can be stably stored for more than one year under cool, sealed, and dry conditions even without nitrogen, and the performance indicators of the liquid and the solid are stable.
[0006] The second object of the present invention is to provide a UV resin having UV and wet heat curing properties prepared by the above method, which can be generally used in various UV coatings, inks, and glues, and can directly provide adhesion to difficult-to-attach substrates.
[0007] The third object of the present invention is to provide the use of the UV resin with UV and wet heat curing properties prepared by the above method in the preparation of new energy vehicle battery insulating coatings, inks, and glues.
[0008] Technical solution: The method for preparing a UV resin having UV and wet heat curing properties of the present invention specifically comprises the following steps:
[0009] S1: Add terminal hydroxyl acrylate monomer, polymerization inhibitor and antioxidant to the reactor, and stir until the solid is completely dissolved; quickly heat up to 100-110°C, start the vacuum system, and maintain full vacuum dehydration for 1-3 hours;
[0010] S2: After dehydration is completed, the temperature is quickly lowered to 35-50°C, and diisocyanate monomer is drawn in. After the addition is completed, the heating is started and the temperature is slowly raised to 60-70°C. The heating is turned off, and the temperature is slowly raised to 80-85°C by the reaction exotherm. The first stage of heat preservation reaction is carried out for 1-3 hours, and a slight negative pressure (-0.005 to -0.01Mpa) is maintained during the process. Within the first stage of heat preservation time range, water vapor is introduced in batches to activate the polyurea and biuret reactions. The system will experience a rapid temperature rise phenomenon, and then it is cooled and the temperature is always controlled at 80-85°C.
[0011] S3: Then the temperature is controlled at 80-88°C, and the second stage of heat preservation reaction is carried out for 2-4 hours. Starting from the second stage of heat preservation for 2h, samples are taken every 0.5h to monitor NCO%. When NCO% <9.1%, the heating is turned off, and the system by-products are removed under slight negative pressure, and then the temperature is lowered to 50-60°C, filtered, and discharged; the product is collected to obtain a UV resin with UV and wet heat curing properties.
[0012] 4. Further, as a preferred embodiment, the terminal hydroxyl-containing monomer in step S1 is one or more of hydroxy acrylate HEA, hydroxy methacrylate HEMA, hydroxy acrylate HEA, and hydroxy acrylate HEA;
[0013] Or the terminal hydroxyl monomer is one or more of hydroxy acrylate HEA, hydroxy methacrylate HEMA, hydroxy acrylate HEA, and the ring-opening unit alcohol of hydroxy acrylate HEA and caprolactone;
[0014] Or the terminal hydroxyl monomer is one or more of (meth) acrylic acid and monofunctional epoxy reactive diluent ring-opening unit alcohol, (meth) acrylic acid and oxabutane / epoxide hexacyclic prepolymer, or (methyl) aziridine and PETA product.
[0015] Furthermore, as a preferred embodiment, the polymerization inhibitor in step S1 is one or more of p-hydroxyanisole, tert-butylhydroquinone, and p-tert-butylcatechol, and the addition amount thereof is 0.01% to 0.05% of the total mass of the system.
[0016] Furthermore, as a preferred embodiment, the antioxidant in step S1 is 2,6-di-tert-butyl-4-methylphenol; and its addition amount is 0.1% to 0.5% of the total mass of the system.
[0017] Further, as a preferred embodiment, the diisocyanate monomer in step S2 mainly refers to aliphatic, alicyclic, or saturated linear hydrocarbon chain type diisocyanates with weather-resistant structures, for example, isophorone diisocyanate (IPDI), dicyclohexylmethane diisocyanate (HMDI), 1,4-cyclohexane diisocyanate (CHDI), meta-xylylene diisocyanate (XDI), dimer acid diisocyanate (DDI, bio-based type), cyclohexane hexamethylene diisocyanate (CDI), diisocyanate (DDI, bio-based type ... (HDI), naphthyl diisocyanate (NDI, high temperature resistant type) and one or more thereof; also includes toluene diisocyanate (TID), diphenyl cyclomethane diisocyanate (MDI) and other diisocyanates that are not resistant to yellowing but have low costs and one or more thereof; also includes polyphenyl polymethylene polyisocyanate (PAPI), polymeric MDI (including PM200, PM400, PM600, PM700), TDI trimer, HDI trimer, IPDI trimer and other polyisocyanates;
[0018] Under working conditions where weather resistance and yellowing resistance are not required, relatively cheap TDI, MDI, polymerized MDI, etc. are usually selected to synthesize with hydroxy (meth) acrylate or hydroxy (methacrylate and caprolactone, epoxy ring-opening monomer);
[0019] Under the conditions of weather resistance and yellowing resistance, HDI, IPDI, HMDI, etc. are usually selected to synthesize with hydroxy (meth) acrylate or hydroxy (methacrylate and caprolactone, epoxy ring-opening monomer);
[0020] In the case of high temperature resistance (above 180°C) and low temperature resistance (below -40°C), XDI, CHDI and hydroxy (meth) acrylate or hydroxy (methacrylate and caprolactone, epoxy ring-opening monomer) are selected for synthesis;
[0021] In military industry, major equipment, special clothing (waterproof and oilproof, infrared stealth), high-performance axles, etc., NDI, DDI, XDI and hydroxy (meth) acrylate or hydroxy (methacrylate and caprolactone, epoxy ring-opening monomer) are selected for synthesis;
[0022] Furthermore, as a key operation for producing biuret and polyurea in the present application, the negative pressure range in step S2 is -0.01Mpa to -0.095Mpa; the slight negative pressure range in step S3 is between -0.005Mpa and -0..01Mpa;
[0023] Step S2: introducing water vapor 2-3 times, each time introducing an amount of 0.01% to 0.02% of the total mass of the reaction system; during the introduction of water vapor, the system is at normal pressure 1.0 MPa or slightly positive pressure 0.01 MPa; each introduction lasts for 1-3 seconds, with an interval of 5-10 minutes.
[0024] Furthermore, as a more preferred embodiment, the molar ratio of the terminal hydroxyl group-containing monomer to the diisocyanate monomer added in the system is 1:2-4.
[0025] The present invention also provides a UV resin having UV and wet heat curing properties prepared by the above preparation method, which comprises the following structural formula:
[0026]
[0027]
[0028] In the structural formula: R1 is CH3 or H; R2 is O or NH; R3 is CH(2-4); and R4 contains a cyclohexyl structure block.
[0029] The present invention also provides the use of the UV resin with UV and wet heat curing properties prepared by the above method in the preparation of new energy vehicle battery insulating coatings, inks, and glues.
[0030] Beneficial effects: (1) The present invention provides a new UV resin with UV and wet heat curing properties and a preparation method thereof. The prepared liquid product has low viscosity, is transparent and clear, has a high NCO content in the polymerized state (NCO% = (8-10)%), contains no free isocyanate, has no odor or smell, is non-toxic, complies with EU ROHS requirements, and has not only UV and wet heat curing properties, but also has the properties of secondary thermal initiation / vulcanization or self-curing by adding polyols;
[0031] (2) The preparation method provided by the present invention has a simple process, is safe, environmentally friendly, reliable and stable throughout the production process, does not use a catalyst throughout the process, does not contain heavy metal ions and halogens, does not contain toxic and harmful ingredients, does not use any solvents and EU ROHS banned ingredients, has a short production time, and does not have the risks of gelation, temperature shock, and curing. The product has no residual free isocyanate, only polymerized NCO. The product is stored in a sealed, cool, and dry condition and can be stored stably for a long time even without nitrogen protection. After one year of storage, it was found that the various performance indicators of the liquid state were stable, and the performance indicators of the solidified product of the application formula were stable;
[0032] (3) The UV resin with UV and wet heat curing properties provided by the present invention is both hard and tough, has excellent adhesion to most difficult-to-attach substrates, is resistant to boiling, alcohol and acetone wiping, solvent immersion, battery electrolyte immersion, high gloss, acid, alkali and salt corrosion, high voltage resistance, and Class F high-grade insulation;
[0033] (4) The liquid product prepared by the method provided by the present invention can be generally used for various UV coatings / inks / glue, solve the adhesion problem of difficult-to-attach substrates, solve the curing problem of parts that cannot be or are difficult to reach with UV light, and solve the curing problem of formulations containing opaque pigments / fillers; especially black, white, flame retardant / thermal conductive formulations;
[0034] (5) The UV resin with UV and wet heat curing properties prepared by the method of the present invention can be used to manufacture insulating coatings / inks / glue for new energy vehicle batteries, replacing traditional battery production processes / materials, such as blue film PET, PVC film, PSA tape, etc. Only a single layer of the coating / ink / glue of the present invention is required, which can save a variety of materials and multiple processes, including the accompanying isolation film / plastic / release paper and other consumables, and significantly reduce energy consumption / environmental protection; the coating thickness is only 100±20 microns, which is conducive to reducing the volume and weight of the battery, and the battery is designed and manufactured; on the existing battery production line, high-pressure airless spraying equipment and UV / LED curing equipment are added, and the production efficiency can be increased by more than 10 times with relatively low investment and technical transformation, and the production energy consumption is less than 1 / 10 of the original, with high yield and low consumption, and significant cost reduction and efficiency improvement.
[0035] It has excellent adhesion on aluminum, aluminum alloy, aluminum-magnesium alloy, anodized aluminum, stainless steel, copper, glass, carbon fiber, PET, PC, most plastics and other substrates, is both hard and tough, resistant to impact without cracking or bursting, resistant to bending without cracking or bursting, resistant to boiling, alcohol, electrolyte immersion, corrosion, condensation, F-class advanced insulation, high voltage resistance, IP protection grade up to IP68, flame retardant up to UL-94V0, thermal conductivity greater than 1.5w / mk, providing the insulation, high voltage resistance, flame retardant, thermal conductivity, anti-condensation and other functions required by the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is the infrared spectrum of the UV resin product with UV and wet heat curing properties obtained in Example 1. DETAILED DESCRIPTION
[0037] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] Unless otherwise specified, the materials added in all the examples are commercially available.
[0039] Example 1: First, add HEA126g (1.086mol), MEHQ0.4g, and BHT0.6g into the reaction kettle, quickly heat it to 105°C ± 5°C, start the vacuum system, control the vacuum degree to gradually increase from -0.01MPa to -0.095MPa, and maintain full vacuum dehydration and impurity removal for 1-2h; if this operation is not in place, side reactions or gels are likely to occur during subsequent synthesis;
[0040] After dehydration, the temperature was quickly lowered to 35-45°C, and 244 g (1.1 mol) of IPDI was quickly poured in, with an R value of 2.0;
[0041] Start heating, control the temperature to rise slowly to 60-70℃, turn off heating, use the reaction heat to slowly raise the temperature to 80-85℃, perform micro-cooling as needed, keep the temperature stable at 85℃±2℃, and carry out the first stage of heat preservation for 1-3h;
[0042] During the first stage of heat preservation, a small amount of water vapor is introduced at about 85°C to activate the polyurea or biuret reaction. There will be an obvious rapid temperature rise phenomenon, bubbles will be generated, the volume will expand slightly, and the material will turn from transparent to translucent. Cool as needed and always control the temperature at 82-88°C. Start the vacuum system to remove the carbon dioxide bubbles generated by negative pressure. After about 0.5 hours, it will become transparent and clear again. This indicates that this step is completed and the second stage of heat preservation can be carried out.
[0043] The second stage is to keep warm for 2-4 hours. From the second hour of keeping warm, take samples every 0.5 hours to monitor NCO% (n-butylene diamine method of GB 2409). When NCO% is <9.1%, turn off the heating and remove the by-product carbon dioxide with slight negative pressure; then cool to 50-60℃, filter and discharge to obtain UV resin with UV and wet heat curing properties. The product has a transparent and clear appearance, high gloss (gloss at 60 degrees and 25 degrees is 105-110), viscosity 15000-20000cp / 25℃, NCO% content 8.8-9.1%, and storage stability (sealed dry and cool conditions, no nitrogen, natural storage) is more than 12 months and stable. Curing speed: UV energy above 200mj, lamp distance greater than 50mm, line speed greater than 80m / min, one-time surface curing, placed at natural room temperature, humidity greater than 65%, temperature greater than 30℃, complete curing in 24-48h, hardness 3-4H, impact resistance greater than 1000j, bending resistance test <2T, excellent toughness, both hard and tough, and high adhesion.
[0044] like Figure 1As shown in the figure, it is the infrared spectrum of the UV resin product with UV and wet heat curing properties obtained in this embodiment. It can be seen from the spectrum that the OH peak 3371cm-1 of HEA disappears, NH absorption peaks are generated near 3654cm-1, 3343cm-1, and 3000cm-1, and at the same time, a C=O vibration / stretching absorption peak unique to IPDI type polyurethane is generated at 1500-1700cm-1, and a CN absorption peak is generated at 1000-1300cm-1. The simultaneous appearance of these characteristic peaks indicates that NHCO is generated, the synthesis is successful, and the target product is obtained; in addition, a weak absorption peak appears at 1637cm-1 (downward shift occurs, moving down from 1660-1680cm-1, which is NHCO The strong absorption peak at 1527cm-1 and the weak absorption peaks at 1192cm-1 and 1239cm-1 appear at the same time, indicating the generation of polyurea and biuret; the C=C absorption peak of HEA is dominant at 2954cm-1, superimposed with the methylene absorption peak of IPDI and the CH2 absorption peak of HEA; the carbonyl absorption peak is at 1724cm-1; the strong absorption peak at 2264cm-1 is the residual NCO group, which is caused by the extrapolation of the overall charge of the main chain after the successful synthesis of IPDI, and the increase of the NCO activity distance on the saddle-shaped polycyclic ring of IPDI, which moves up from 2255cm-1; in summary, it is proved that the UV resin with UV and wet heat curing properties is successfully synthesized in this embodiment.
[0045] Embodiment 2:
[0046] Add HEMA132g (1.015mol), MEHQ0.4g, BHT0.6g, IPDI 266.4g (1.2mol) into the reaction kettle, R value 2.36; other process operations are the same as in Example 1; the final product has a transparent and clear appearance, high gloss (gloss at 60 degrees and 25 degrees is 105-110), viscosity 15000-18900cp / 25℃, NCO% content 8.9-9.2%, storage stability (sealed dry and cool conditions, no nitrogen, natural storage) greater than 12 months and stable. Curing speed: UV energy above 150mj, lamp distance greater than 50mm, line speed greater than 80m / min, one-time surface curing, placed at natural room temperature, humidity greater than 65%, temperature greater than 30℃, 24-48h complete curing, hardness 3H, impact resistance greater than 1000j, bending resistance test <2T, both hard and tough, high adhesion.
[0047] Example 3: Add HEA170g (1.349mol), MEHQ0.5g, BHT0.8g, HDI 284g (1.69mol) into the reaction kettle, R value 2.5; process operation is the same as Example 1; the product has a transparent and clear appearance, a viscosity of 12000-16000cp / 25℃, an NCO% content of 8.9-9.1%, and storage stability (sealed dry and cool conditions, no nitrogen, natural storage) is greater than 12 months and stable. Curing speed: UV energy of more than 200mj, lamp distance greater than 50mm, line speed greater than 80m / min, one-time surface curing, placed at natural room temperature, humidity greater than 65%, temperature greater than 30℃, 24-48h complete curing, hardness 2-3H, impact resistance greater than 1500j, bending resistance test <2T, excellent toughness, high adhesion.
[0048] Example 4: Add HEMA198g (1.5mol), MEHQ0.5g, BHT0.8g, HDI 282g (1.68mol) into the reaction kettle, R value 2.24; process operation is the same as Example 1; the product has a transparent and clear appearance, high gloss (gloss at 60 degrees and 25 degrees is 105-110), viscosity 10000-13000cp / 25℃, NCO% content 8.8-8.95%, storage stability (sealed dry and cool conditions, no nitrogen, natural storage) is greater than 12 months and stable. Curing speed: UV400mj or more energy, lamp distance greater than 50mm, line speed greater than 80m / min, one-time machine surface curing, placed at natural room temperature, humidity greater than 65%, temperature greater than 30℃, 24-48h complete curing, hardness 2-3H, impact resistance greater than 1500j, bending resistance test <2T, excellent toughness, high adhesion.
[0049] Example 5: Add HEA151g (1.2mol), MEHQ0.5g, BHT0.8g, HMDI 410g (1.56mol) into the reaction kettle, R value 2.6; process operation is the same as Example 1; the product has a transparent and clear appearance, a viscosity of 15000-20000cp / 25℃, an NCO% content of 9.0-9.3%, and storage stability (sealed dry and cool conditions, no nitrogen, natural storage) is greater than 12 months and stable. Curing speed: UV energy of more than 200mj, lamp distance greater than 50mm, line speed greater than 80m / min, one-time surface curing, placed at natural room temperature, humidity greater than 65%, temperature greater than 30℃, 24-48h complete curing, hardness 3-4H, impact resistance greater than 1000j, bending resistance test <2T, excellent toughness, both hard and tough, high adhesion.
[0050] Example 6: Add HEMA178g (1.35mol), MEHQ0.6g, BHT 1g, HMDI 499g (1.9mol) into the reaction kettle, R value 2.82; process operation is the same as Example 1; the product has a transparent and clear appearance, high gloss (gloss at 60 degrees and 25 degrees is 105-110), viscosity 15000-20000cp / 25℃, NCO% content 9.0-9.3%, storage stability (sealed dry and cool conditions, no nitrogen, natural storage) greater than 12 months and stable. Curing speed: UV200mj or more energy, lamp distance greater than 50mm, line speed greater than 80m / min, one-time machine surface curing, placed at natural room temperature, humidity greater than 65%, temperature greater than 30℃, 24-48h complete curing, hardness 3-4H, impact resistance greater than 1000j, bending resistance test <2T, excellent toughness, both hard and tough, high adhesion.
[0051] For the synthesis formulas and processes of HPA, HPMA, HEA-caprolactone, HEMA-caprolactone, and various other (meth)acrylate hydroxy esters and IPDI, HDI, HMDI, CHDI, DDI, and NDI, the above-mentioned processes and ratio R values are followed to obtain similar high-performance and high-adhesion products.
[0052] Comparative Example 1: (The amounts added in this example are all parts by mass)
[0053] Add 500 parts of polyester diol (hydroxyl equivalent is 500g / mol) to the reaction vessel, heat to 100°C, vacuum dehydrate for 1.5 hours, cool to room temperature, add 0.2 parts of dibutyltin dilaurate, heat up, control the temperature at 45-50°C, drop 275 parts of isophorone diisocyanate, and continue to keep warm for 30 minutes after dripping within 1.5 hours, then add 0.26 parts of p-hydroxyanisole and 2.58 parts of 2,6-di-tert-butyl-4-methylphenol in the reactor, stir until the solid is completely dissolved, heat up, control the temperature at 50-55°C, drop 85 parts of hydroxyethyl acrylate, and continue to keep warm for 30 minutes after dripping within 1 hour, heat up, and keep warm at 68-75°C for 2 hours, the reaction is completed, cool to below 55°C to discharge, and obtain the product of Comparative Example 1. NCO% content 8.0-8.04%. The viscosity is 25000-55000cp / 25℃. It is hard and brittle after curing, but the wet heat curing speed is very slow, and it takes 3-5 days to cure completely, and the adhesion is poor.
[0054] Comparative Example 2: (The amounts added in this example are all parts by mass)
[0055] This comparative example is basically the same as comparative example 1, except that the feedstock is 500 parts of polyether diol (hydroxyl equivalent is 800 g / mol), 0.2 parts of dibutyltin dilaurate, 275 parts of isophorone diisocyanate, 0.26 parts of p-hydroxyanisole, and 2.57 parts of 2,6-di-tert-butyl-4-methylphenol. The product of comparative example 2 is obtained. NCO% content is 8.3%; viscosity is 25000-55000cp / 25℃, hard and brittle after curing, but the wet heat curing speed is very slow, and it takes 4-7 days to fully cure, and the adhesion is poor.
[0056] Comparative tests and findings show that: under the same basic formula and process conditions (different ratios of different hydroxy esters and different isocyanates, different R values, but all within the range of 2-4), whenever a catalyst is added, such as dibutyltin dilaurate or organic bismuth, etc., with a dosage of 1 to 5 parts per thousand, no matter which hydroxy ester and isocyanate, the reaction is very violent, and the process is difficult to control. It requires strong cooling with cooling water, long cooling, and must be changed to a dripping process. The products have no storage stability, and will gel in 3-7 days even if sealed, nitrogen-filled, cool, and dry, and the longest will not exceed 30 days. This means that catalysts cannot be used in this type of synthesis. Eliminate;
[0057] Under the same basic formula and process conditions, without adding a catalyst, only eliminating water, the process is relatively easy to control and can be cooled as needed, but the product does not contain polyurea and biuret, the solidified material is very hard (hardness greater than 4H, usually up to 5-6H), brittle, not impact-resistant, and has no toughness.
[0058] In summary, it was found that the NCO% surplus is greater than 10%, and the product viscosity is low, generally not higher than 9000cp / 25℃, usually 5500-8500cp / 25℃. It is hard and brittle after curing and cannot be used alone. It usually needs to be compounded with other polyol resins or UV resins with good flexibility. When used with polyols, it can only be a two-component formula, and the window opening time (operation time) is 8-12h at room temperature. The performance is comparable to that of traditional two-component solvent-based PU products, and the service life is doubled. When used with UV resins with good flexibility, the performance of the cured film decreases rapidly. As the amount of UV resin with good flexibility increases, the strength decreases, the hardness decreases, and the chemical and water resistance decreases.
[0059] The NCO% residue is less than 8.5%, and the product viscosity is high, generally greater than 25000cp / 25℃, usually between 25000-55000cp / 25℃. It is hard and brittle after curing, but the wet heat curing speed is very slow, usually taking 3-7 days to completely cure. As the NCO% residue decreases, the curing time will increase to 15 days. When NCO% is less than 5%, the performance of the cured product decreases, the adhesion is poor, and the performance is similar to that of ordinary polyurethane acrylate UV resins with more than 3 functionalities. If a catalyst is added to these formulas, there is no storage stability, and under natural conditions, even if it is sealed, cool, dry, and ventilated with nitrogen, it will not exceed 3 months at most, and usually within 1 month.
[0060] The UV resin with UV and wet heat curing properties prepared in this application scheme can be used to manufacture insulating coatings on the aluminum-based surface of the lithium battery shell of new energy vehicles. The specific preparation formula is as follows:
[0061] 100g of UV resin with UV and moisture heat curing properties;
[0062] Low-viscosity polyester PUA (polyurethane acrylate) 5-10g;
[0063] Modified epoxy acrylate EA 10-20g;
[0064] Cyclotrimethylolpropane formal acrylate CTFA 5-10g;
[0065] Isoborneol acrylate IBOA 10-15 g;
[0066] Hydroxyethyl methacrylate HEMA 5-10g;
[0067] Reactive UV flame retardant resin 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide 1-3g;
[0068] Super wetting dispersant TEG5101 1-3g;
[0069] Latent promoter DMP-30 1-3g;
[0070] PU modified epoxy resin 3-5g;
[0071] 3,4-Epoxycyclohexylmethyl 3,4-epoxycyclohexylcarboxylate 5-10 g;
[0072] Photoinitiator 2,4,6-trimethylbenzoylphenylphosphonic acid ethyl ester 3-6g;
[0073] Photoinitiator hydroxycyclohexane phenone 4-6g;
[0074] Ultrafine spherical corundum thermal conductive powder 40-80g;
[0075] Reactive UV flame retardant resin THPO trishydroxymethylphosphine oxide 5-10g;
[0076] Antioxidant bis(2-morpholine diethyl) ether 1-5g;
[0077] BYK defoamer 1-2g;
[0078] The above formula can be used to prepare the insulating coating for the aluminum-based surface of the lithium battery shell of new energy vehicles. The specific properties are as follows:
[0079] Liquid indicators: viscosity 1500-5500cp / 25℃, white semi-matte liquid, with a slight odor of borneol, non-toxic and harmless, no banned substances; high-pressure airless spray thickness (maintain 40-50℃, normal room temperature / humidity of workpiece and environment) 80-120 microns; silk screen <100 mesh, 50-80 microns thickness; excellent construction processability, no sag, good leveling.
[0080] Curing: UV or LED, energy 600-2000mj, illumination distance 50-20mm, line speed 50-200m / min, one-time drying, UV / LED curing is good; fully cured in 2-4h at 60-80℃, relative humidity 65-85%; fully cured in 2-3 days at room temperature, 20-40℃, relative humidity 50-80% in natural environment;
[0081] Test results of cured product performance: Directly attached to the aluminum substrate of lithium battery shell (0 grade or 5B, hundred grid method); hardness 2-3H (pencil hardness); toughness (GB method, bend 4 times, aluminum plate breaks, no cracking or film bursting, <2T); impact resistance (GB, >1500j, no cracking or film bursting); boiling resistance (>2h / 100℃); alcohol resistance (anhydrous alcohol, 80℃>0.5h); electrolyte immersion resistance (electrolyte 45℃>30 days); corrosion resistance (GB method, acid, alkali and salt accelerated test>90d); anti-condensation (environment <5℃, humidity above 85% / water vapor humidity>50℃, no abnormality for 30d); F-class advanced insulation (GB method); high voltage resistance (>5Kv / mm); IP protection level reaches IP68; flame retardant reaches UL-94V0 level; thermal conductivity>1.5w / mk; double 85 test (GB method, >90 days);
[0082] From the above data, we can see that it can meet the stringent testing and performance requirements put forward by customers and provide the insulation, high voltage resistance, flame retardancy, thermal conductivity, anti-condensation and other functions required by lithium batteries.
[0083] The UV resin with UV and wet heat curing properties prepared in the present application can also be used to make varnish for glass substrates. The specific preparation formula is as follows:
[0084] 100g of UV resin with UV and moisture heat curing properties;
[0085] Low-viscosity polyester PUA (polyurethane acrylate) 5-10g;
[0086] Latent promoter DMP-30 1-3g;
[0087] Isoborneol acrylate IBOA 10-15 g;
[0088] Hydroxyethyl methacrylate HEMA 10-15g;
[0089] BYK defoamer 1-2g;
[0090] Reactive UV flame retardant resin 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide 5-10g;
[0091] PU modified epoxy resin 3-5g;
[0092] 3,4-Epoxycyclohexylmethyl 3,4-epoxycyclohexylcarboxylate 5-10 g;
[0093] Photoinitiator 2,4,6-trimethylbenzoylphenylphosphonic acid ethyl ester 3-6g;
[0094] Photoinitiator hydroxycyclohexane phenone 4-6g;
[0095] Reactive UV flame retardant resin THPO trishydroxymethylphosphine oxide 5-10g;
[0096] Antioxidant bis(2-morpholine diethyl) ether 1-5g;
[0097] The above formula can be used to prepare varnish for glass substrates, and the specific properties are as follows:
[0098] Liquid indicators: viscosity 1000-3500cp / 25℃, slight odor of isoborneol, non-toxic and harmless, no banned substances; high-pressure airless spray thickness (maintain 40-50℃, normal room temperature / humidity of workpiece and environment) 30-90 microns; silk screen <100 mesh, 30-60 microns thickness; excellent construction processability, no sag, good leveling.
[0099] Curing: UV or LED, energy 500-1500mj, illumination distance 50-20mm, line speed 50-100m / min, one-time drying, UV / LED curing is good; fully cured in 2-4h at 60-80℃, relative humidity 65-85%; fully cured in 2-3 days at room temperature, 20-40℃, relative humidity 50-80% in natural environment;
[0100] Test results of cured product performance: Directly adhered to glass substrate (grade 0 or 5B, hundred grid method); hardness 2-3H (pencil hardness); toughness (GB method, <2T); impact resistance (GB>1000j); boiling resistance (>2h / 100℃); alcohol resistance (anhydrous alcohol, 80℃>0.5h); flame retardant up to UL-94V0 level; double 85 test (>30 days); short-term high temperature resistance (>240℃, 5min); long-term working temperature (-20 to 180℃);
[0101] From the above data, it can be seen that it meets the stringent testing and performance requirements put forward by customers, can provide the adhesion, high and low temperature resistance, flame retardancy, and double 85 requirements required by the glass base, directly adheres to the glass base, has both hardness and toughness, is wear-resistant and scratch-resistant, and is resistant to high and low temperatures. It can be used for glass window inks and coatings / inks for gas stove glass.
[0102] The UV resin with UV and wet heat curing properties prepared in the present application can also be used to manufacture coatings for BOPP substrates. The specific preparation formula is as follows:
[0103] 100g of UV resin with UV and moisture heat curing properties;
[0104] Low-viscosity polyester PUA (polyurethane acrylate) 5-10g;
[0105] Latent promoter DMP-30 1-3g;
[0106] Isoborneol acrylate IBOA 10-15 g;
[0107] Hydroxyethyl methacrylate HEMA 5-10g;
[0108] BYK defoamer 1-2g;
[0109] Super wetting dispersant TEG5101 1-3g;
[0110] PU modified epoxy resin 3-5g;
[0111] Linear phenolic type EA 30-60g;
[0112] Photoinitiator 2,4,6-trimethylbenzoylphenylphosphonic acid ethyl ester 3-6g;
[0113] Photoinitiator hydroxycyclohexane phenone 4-6g;
[0114] Antioxidant bis(2-morpholine diethyl) ether 1-5g;
[0115] UV color paste 17-53g;
[0116] The above formula can be used to prepare ink for BOPP substrate, the specific properties are as follows:
[0117] Liquid indicators: viscosity 1500-5500cp / 25℃, slight odor of isoborneol, non-toxic and harmless, no banned substances; screen printing thickness 3-20 microns; excellent construction processability, no ink flying, no sticking to the mesh.
[0118] Curing: UV or LED, energy 200-1000mj, illumination distance 50-20mm, line speed 70-200m / min, one-time drying, good UV / LED curing, good adhesion; fully cured in 2-4h at 60-80℃, relative humidity 65-85%; fully cured in 1 day at room temperature in a natural environment at 20-40℃, relative humidity 50-80%;
[0119] Test results of cured product performance: Directly attached to BOPP substrate (3M tape pulling); Hardness 1H (pencil hardness); The film does not break, crack, or fall off when rubbed; Boiling resistance (>1h / 100℃); Alcohol resistance (no abnormality after wiping 200 times); High pressure and high temperature cooking (3-5kgf, no abnormality for 0.5h);
[0120] From the above data, we can see that if the BOPP test requirements are met, BOPP ink can be used for food packaging bags, mineral water bottle printing, beverage bottle printing, cola packaging printing, etc.
[0121] The UV resin with UV and wet heat curing properties prepared in the present application can also be used to make carbon fiber or aramid fiber ink or its cloth-based impregnation coating, or its cloth layer adhesive. The specific preparation formula is as follows:
[0122] 100g of UV resin with UV and moisture heat curing properties;
[0123] Low-viscosity polyester PUA (polyurethane acrylate) 5-10g;
[0124] Antioxidant bis(2-morpholine diethyl) ether 1-5g;
[0125] Isoborneol acrylate IBOA 5-10 g;
[0126] Hydroxyethyl methacrylate HEMA 10-15g;
[0127] BYK defoamer 1-2g;
[0128] Cyclotrimethylolpropane formal acrylate 20-35g;
[0129] 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide 3-5 g;
[0130] Linear phenolic type EA 50-90g;
[0131] Photoinitiator 2,4,6-trimethylbenzoylphenylphosphonic acid ethyl ester 3-6g;
[0132] Photoinitiator hydroxycyclohexane phenone 4-6g;
[0133] THPO trishydroxymethylphosphine oxide 5-10g;
[0134] PU modified epoxy resin 5-10g;
[0135] The above formula can be used to prepare the ink for manufacturing carbon fiber or aramid fiber or the impregnation coating of its cloth base, or the adhesive of its cloth layer, and the specific properties are as follows:
[0136] Liquid indicators: viscosity 200-600cp / 40℃, slight odor of isoborneol, non-toxic and harmless, no banned substances; meets the comprehensive process requirements of infiltration, spraying and silk-screen printing.
[0137] Curing: UV or LED, energy 1000-3000mj, illumination distance 20-30mm, line speed 50-200m / min, one-time drying, good UV / LED curing, good adhesion; fully cured in 2-4h at 60-80℃, relative humidity 65-85%; fully cured in 1 day at room temperature in a natural environment at 20-40℃, relative humidity 50-80%;
[0138] Test results of cured product performance: Directly attached to carbon fiber and aramid fiber base (3M tape pulling); hardness 2H (pencil hardness); film rubbing does not expose the film, crack, or fall off; boiling resistance (>1h / 100℃); alcohol resistance (no abnormality after wiping 200 times); ink penetration rate>30%; flame retardant UL-94V0 level; high and low temperature resistance -40-180℃; insulation grade F; high voltage resistance 5KV; inter-layer adhesion>26N, shear force>22N; tensile strength increased by 10-30%, and elongation at break was not affected;
[0139] From the above data, it can be seen that it meets the test requirements of carbon fiber and aramid fiber, and can be used for carbon fiber and aramid fiber inks, or impregnation coatings of their cloth bases, or bonding of their cloth layers. It can be used in the production of various lightweight and high-strength composite materials, such as drone wings, vehicle parts, fishing rods, etc.
[0140] The UV resin with UV and wet heat curing properties prepared in the present application can also be used to make acrylic / PET bonding OCA glue. The specific preparation formula is as follows:
[0141] 100g of UV resin with UV and moisture heat curing properties;
[0142] Crystalline PUA 10-20g;
[0143] Antioxidant bis(2-morpholine diethyl) ether 1-5g;
[0144] Isoborneol acrylate IBOA 10-30g;
[0145] Hydroxyethyl methacrylate HEMA 20-35g;
[0146] OCA (liquid optical adhesive) resin 50-90g;
[0147] Modified rosin 20-30g;
[0148] Photoinitiator 2,4,6-trimethylbenzoylphenylphosphonic acid ethyl ester 3-5g;
[0149] Photoinitiator hydroxycyclohexane phenone 3-5g;
[0150] SBR (styrene butadiene) liquid rubber 10-20g;
[0151] The above formula can be used to prepare the OCA adhesive for making acrylic / PET, and the specific properties are as follows:
[0152] Test results: Adhesion (>32N), shear force (>23N), initial adhesion (>15N), and lasting adhesion (>30N).
[0153] The product of the invention is used for UV adhesives and UV tapes, such as non-impact adhesives, electronic UV protective adhesives, UV structural adhesives, UV tapes, OCA adhesives, etc., and has excellent bonding performance between acrylic, PET, glass, and with metals, plastics, copper, stainless steel, aluminum and aluminum alloys, and nylon.
[0154] The UV resin with UV and wet heat curing properties prepared by the method of the present invention can be used to manufacture insulating coatings / inks / glue for new energy vehicle batteries, replacing traditional battery production processes / materials, such as blue film PET, PVC film, PSA tape, etc., only a single layer of the coating / ink / glue of the present invention is needed, and multiple materials and multiple processes, including accompanying consumables such as isolation films / plastics / release paper, etc., can be omitted, and energy saving / environmental protection is obvious; the coating thickness is only 100±20 microns, which is conducive to reducing the volume and weight of the battery, and the battery special-shaped is designable and manufacturable; on the existing battery production line, high-pressure airless spraying equipment and UV / LED curing equipment are added, and the production efficiency can be improved by more than 10 times with relatively low investment and technical transformation, and the production energy consumption is less than 1 / 10 of the original, with high yield and low consumption, and obvious cost reduction and efficiency improvement.
[0155] It has excellent adhesion on aluminum, aluminum alloy, aluminum-magnesium alloy, anodized aluminum, stainless steel, copper, glass, carbon fiber, PET, PC, most plastics and other substrates, is both hard and tough, resistant to impact without cracking or bursting, resistant to bending without cracking or bursting, resistant to boiling, alcohol, electrolyte immersion, corrosion, condensation, F-class advanced insulation, high voltage resistance, IP protection grade up to IP68, flame retardant up to UL-94V0, thermal conductivity greater than 1.5w / mk, providing the insulation, high voltage resistance, flame retardant, thermal conductivity, anti-condensation and other functions required by the battery.
[0156] As described above, although the present invention has been shown and described with reference to specific preferred embodiments, it should not be construed as limiting the present invention itself. Various changes in form and details may be made without departing from the spirit and scope of the present invention as defined in the appended claims.
Claims
1. A method for preparing a UV resin having UV and wet heat curing properties, characterized in that The steps include: S1: Add terminal hydroxyl monomer, polymerization inhibitor and antioxidant to the reactor, and stir until the solid is completely dissolved; quickly heat up to 100-110°C, start the vacuum system, and maintain full vacuum dehydration for 1-3 hours; S2: After dehydration is completed, the temperature is quickly lowered to 35-50°C, and diisocyanate monomer is pumped in. After the addition is completed, the heating is started and the temperature is slowly raised to 60-70°C. The heating is turned off, and the temperature is slowly raised to 80-85°C by the reaction exotherm. The first stage of heat preservation reaction is carried out for 1-3 hours, and negative pressure conditions are maintained during the process. Within the first stage of heat preservation time range, water vapor is introduced in batches to activate the polyurea and biuret reactions. The system will experience a rapid temperature rise phenomenon, and then it is cooled and the temperature is always controlled at 80-85°C. S3: Then the temperature is controlled at 80-88°C, and the second stage of heat preservation reaction is carried out for 2-4 hours. Starting from the second stage of heat preservation for 2 hours, samples are taken every 0.5 hours to monitor NCO%. When NCO% is <9.1%, the heating is turned off, the system by-products are removed under slight negative pressure, and then the temperature is lowered to 50-60°C, filtered, and discharged; The collected product is a UV resin having UV and wet heat curing properties.
2. The method for preparing a UV resin having UV and wet heat curing properties according to claim 1, characterized in that: The terminal hydroxyl-containing monomer in step S1 is one or more of a single terminal hydroxyl-containing acrylate monomer or a prepolymer thereof.
3. The method for preparing a UV resin having UV and wet heat curing properties according to claim 2, characterized in that: The terminal hydroxyl-containing monomer in step S1 is one or more of hydroxy acrylate HEA, hydroxy methacrylate HEMA, hydroxy acrylate HEA, and hydroxy acrylate HEA; Or the terminal hydroxyl monomer is one or more of hydroxy acrylate HEA, hydroxy methacrylate HEMA, hydroxy acrylate HEA, and the ring-opening unit alcohol of hydroxy acrylate HEA and caprolactone; Or the terminal hydroxyl monomer is one or more of (meth) acrylic acid and monofunctional epoxy reactive diluent ring-opening unit alcohol, (meth) acrylic acid and oxabutane / epoxide hexacyclic prepolymer, or (methyl) aziridine and PETA product.
4. The method for preparing a UV resin having UV and wet heat curing properties according to claim 1, characterized in that: The polymerization inhibitor in step S1 is one or more of p-hydroxyanisole, tert-butylhydroquinone, and p-tert-butylcatechol, and the addition amount thereof is 0.01% to 0.05% of the total mass of the system.
5. The method for preparing a UV resin having UV and wet heat curing properties according to claim 1, characterized in that: The antioxidant in step S1 is 2,6-di-tert-butyl-4-methylphenol; the added amount thereof is 0.1% to 0.5% of the total mass of the system.
6. The method for preparing a UV resin having UV and wet heat curing properties according to claim 1, characterized in that: The diisocyanate monomer in step S2 is one or more of isophorone diisocyanate, dicyclohexylmethane diisocyanate, 1,4-cyclohexane diisocyanate, m-xylylene diisocyanate, cyclohexane dimethylene diisocyanate, naphthyl diisocyanate, toluene diisocyanate, diphenylcyclomethane diisocyanate, and polyphenylene polymethylene polyisocyanate.
7. The method for preparing a UV resin having UV and wet heat curing properties according to claim 1, characterized in that: The negative pressure range in step S2 is -0.01Mpa to -0.095Mpa; the slight negative pressure range in step S3 is between 1.0Mpa and -0.01Mpa; Step S2: introducing water vapor 2-3 times, each time introducing an amount of 0.01% to 0.02% of the total mass of the reaction system; during the introduction of water vapor, the system is at a normal pressure of 0.1 MPa or a slight positive pressure of 0.01 MPa; each introduction lasts for 1-3 seconds, with an interval of 5-10 minutes.
8. The method for preparing a UV resin having UV and wet heat curing properties according to claim 1, characterized in that: The molar ratio of the terminal hydroxyl monomer to the diisocyanate monomer in the system is 1:2-4.
9. A UV resin having UV and moisture heat curing properties obtained by the method for preparing a UV resin having UV and moisture heat curing properties according to any one of claims 1 to 7.
10. Use of the UV resin having UV and wet heat curing properties in claim 8 in preparing insulating coatings, inks and glues for new energy vehicle batteries.
Citation Information
Patent Citations
Method for preparing polyisocyanate containing biuret
CN103724234A
Method of preparing hexamethylene diisocyanate biuret through water vapor method
CN105348486A
Method for producing radiation-curable urethane (meth)acrylates
CN107075074A
Photo-thermal / thermo-optical dual-cured resin, and preparation method and application thereof
CN113248683A
Coating agents which can be hardened by addition of isocyanate groups as well as by radiation-induced addition of activated c-c double covalent bonds