Self-repairing organic silicon heat-conducting gel and preparation method thereof

By using the self-healing mechanism of metal coordination bonds in thermal management materials, the use of polydimethylsiloxane thiocyanide and boron nitride thiocyanide to form a reversible complex with metal salts, the traditional thermal management materials are solved. The problem of damage during long-term use has achieved high thermal conductivity and self-healing efficiency of silicone thermal gels, which simplifies the preparation process and is suitable for large-scale production.

CN119119745APending Publication Date: 2024-12-13GUANGCHANG LIHUA TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411221129.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-12-13

AI Technical Summary

Technical Problem

Traditional thermal management materials may experience mechanical damage under the dual effects of long-term use and internal stress, which weakens their thermal conductivity, and the preparation process of existing self-healing thermal management materials is complicated.

Method used

Using a self-healing mechanism based on metal coordination bonds, a dynamic reversible thiocyano metal salt complex is formed with metal salt through polydimethylsiloxane thiocyanide and boron nitride thiocyanide and metal salt, and the self-healing characteristics are prepared. Thermal conductivity gel simplifies the preparation process and improves thermal conductivity.

Benefits of technology

It realizes a self-healing silicone thermal conductivity gel with a thermal conductivity greater than 2.5W/(m·K) and a room temperature self-repair efficiency greater than 95%, which is suitable for industrial production and large-scale manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119119745A_ABST
    Figure CN119119745A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of thermal management composite materials, and particularly relates to self-repairing organic silicon heat-conducting gel and a preparation method thereof. The self-repairing organic silicon heat-conducting gel is prepared from thiocyanic polydimethylsiloxane, thiocyanic boron nitride and metal salt, wherein thiocyano groups of the thiocyanic polydimethylsiloxane and the thiocyanic boron nitride and the metal salt can form a dynamic reversible thiocyano metal salt complex to realize self-repairing. The preparation method comprises the following steps: performing thiocyano group modification on polydimethylsiloxane and boron nitride respectively, and mixing the modified polydimethylsiloxane and boron nitride with metal salt to form a dynamic reversible thiocyano group metal salt complex. A brand new solution is provided for the self-repairing heat-conducting gel, the heat conductivity coefficient of the prepared heat-conducting gel is larger than 2.5 W / (m.K), the room-temperature self-repairing efficiency is larger than 95%, and the preparation method is not high in equipment requirement, easy to operate and capable of being used for large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of thermal management composite materials, and in particular relates to a self-repairing organic silicon thermally conductive gel and a preparation method thereof. Background Art

[0002] With the rapid development of electronic technology, electronic devices are becoming more and more compact, and the integration of their internal components is increasing. In these small spaces, high-frequency electronic components quickly generate a lot of heat, which puts higher heat dissipation requirements on thermal interface materials. Although silicone thermal interface materials perform well in thermal management, they may also suffer mechanical damage under the dual effects of long-term use and internal stress, thereby weakening their thermal conductivity and posing a potential threat to device performance. In order to meet this challenge, the development of self-healing thermal management materials is particularly critical. Such materials can repair internal damage during operation and quickly restore their thermal conductivity, thereby ensuring the stable operation of electronic equipment.

[0003] Self-healing materials usually benefit from the reversible interaction forces introduced in their cross-linked networks, which give the materials the ability to self-repair. Self-healing mechanisms are mainly divided into two categories: reversible covalent bonds and reversible non-covalent bonds. When a material encounters mechanical damage, its internal reversible bonds can break by themselves without external intervention or under specific stimulation, and re-form in the damaged area, thereby rebuilding the material network structure and restoring its original performance. At present, the developed self-healing materials are mainly constructed through hydrogen bonds, Si-O-Ti bonds, borate bonds, disulfide bonds, etc. The thermal conductive gel constructed by these dynamic bonds can achieve excellent self-healing properties, but its preparation process is relatively complicated. For example, the hydrogen bond between the carboxyl group and the amino group requires the simultaneous preparation of raw materials containing carboxyl groups and amino groups, and thermal conductive fillers need to be added to ensure high thermal conductivity. Summary of the invention

[0004] In view of this, the purpose of the present invention is to provide a self-healing silicone thermal conductive gel and a preparation method thereof, in view of the fact that traditional thermal management materials may suffer mechanical damage under the dual effects of long-term use and internal stress, thereby weakening their thermal conductivity and posing a potential threat to equipment performance, as well as the relatively complex preparation of existing self-healing thermal management materials.

[0005] Specifically, the present invention proposes a self-healing mechanism based on metal coordination bonds to address the defects of existing materials, and is used to prepare a thermally conductive gel with self-healing properties. The thermally conductive gel is directly modified by a silane coupling agent containing a thiocyanate group on the silicone matrix and the thermally conductive filler at the same time, and then coordinated with a metal salt. The design concept of this material not only constructs a composite matrix network that can respond quickly to damage and maintain long-term durability, but also facilitates the introduction of boron nitride fillers with high thermal conductivity, giving the material high thermal conductivity and repair efficiency. In addition, the present invention is simple and easy to prepare, environmentally friendly, and very suitable for industrial continuous production and large-scale manufacturing.

[0006] Furthermore, the present invention first modifies polydimethylsiloxane and boron nitride with thiocyanate groups, and then mixes them with metal salts to form a dynamically reversible thiocyanate metal salt complex. The present invention utilizes the thiocyanate groups of thiocyanated polydimethylsiloxane and thiocyanated boron nitride to form a dynamically reversible thiocyanate metal salt complex with metal salts to achieve self-repairing, and improves the thermal conductivity by thiocyanated boron nitride. The thermal conductivity of the prepared thermally conductive gel is greater than 2.5W / (m·K), and the room temperature self-repairing efficiency is greater than 95%.

[0007] Specifically, the structure of the thiocyanate metal salt complex formed by the thiocyanate group of thiocyanate polydimethylsiloxane and thiocyanate boron nitride and the metal salt is as follows:

[0008]

[0009] In order to achieve the above object, the present invention adopts the following technical solution:

[0010] The first technical purpose of the present invention is to provide a self-repairing silicone thermally conductive gel, which comprises the following components in parts by weight: 50-100 parts of thiocyanate polydimethylsiloxane, 30-80 parts of thiocyanate boron nitride, and 5-20 parts of a metal salt;

[0011] The thiocyanate group of the thiocyanate polydimethylsiloxane can form a thiocyanate metal salt complex with a metal salt;

[0012] The thiocyanate group of the thiocyanated boron nitride can form a thiocyanate metal salt complex with a metal salt.

[0013] Furthermore, the structural formula of the polydimethylsiloxane thiocyanate is shown in Formula I:

[0014]

[0015] Furthermore, the structural formula of the boron nitride thiocyanate is shown in Formula II:

[0016]

[0017] Furthermore, the metal salt is one or more combinations of copper chloride, copper sulfate, copper nitrate, zinc chloride, zinc sulfate, zinc nitrate, nickel chloride, nickel sulfate, nickel nitrate, ferric chloride, ferric sulfate, ferric nitrate, manganese chloride, manganese sulfate, and manganese nitrate.

[0018] It should be noted that the above further beneficial effect is that the thiocyanated polydimethylsiloxane and the thiocyanated boron nitride can form a thiocyanate metal salt complex with the metal salt, thereby obtaining self-healing properties; at the same time, the addition of thiocyanated boron nitride can also improve the thermal conductivity of the system.

[0019] The second technical purpose of the present invention is to provide a method for preparing the self-repairing silicone thermally conductive gel as described above, which specifically comprises the following steps:

[0020] The polydimethylsiloxane thiocyanate, boron nitride thiocyanate and metal salt are mixed in a planetary mixer for 5 to 60 minutes, and then vacuum degassing is performed until there are no bubbles, poured into a polytetrafluoroethylene mold, placed in a vacuum drying oven at 80 to 100° C. for reaction for 1 to 2 hours, and then at 100 to 120° C. for reaction for 2 to 4 hours to obtain the self-healing silicone thermal conductive gel.

[0021] Optionally, the thiocyanate polydimethylsiloxane is obtained by first subjecting polydimethylsiloxane to plasma treatment and then to modification with 3-thiocyanatepropyltriethoxysilane; the thiocyanate boron nitride is obtained by dispersing and exfoliating hexagonal boron nitride to obtain boron nitride nanosheets, and then modifying the boron nitride nanosheets with 3-thiocyanatepropyltriethoxysilane.

[0022] Furthermore, the preparation method of the above-mentioned thiocyanate polydimethylsiloxane specifically comprises the following steps:

[0023] P1. Placing polydimethylsiloxane in a plasma cleaning device, selecting oxygen as a process gas, adjusting the pressure range to be 25 to 135 Pa, and treating for 15 to 60 seconds to obtain hydroxylated polydimethylsiloxane, wherein the viscosity of the polydimethylsiloxane at 25° C. is 5000 to 20000 mPa·s;

[0024] P2. Add the above hydroxylated polydimethylsiloxane and 3-thiocyanatopropyltriethoxysilane into acetone, and stir the mixture at 40-80°C at a speed of 300-1000 rpm for 12-24 hours, wherein the mass of 3-thiocyanatopropyltriethoxysilane is 1%-5% of the hydroxylated polydimethylsiloxane, and the mass of acetone is 50-200 times that of the hydroxylated polydimethylsiloxane; after the reaction is completed, remove the solvent by rotary evaporation at 40-80°C to obtain the thiocyanate polydimethylsiloxane.

[0025] Furthermore, the preparation method of the above-mentioned boron nitride thiocyanate specifically comprises the following steps:

[0026] BN1, dispersing hexagonal boron nitride powder in a mixed solution of isopropanol and deionized water, and ultrasonically exfoliating for 12 to 24 hours under 100 to 500W ultrasound, wherein the volume ratio of isopropanol to deionized water is 1:1, and the mass ratio of hexagonal boron nitride powder to deionized water is 0.05 to 0.2;

[0027] BN2, the dispersion obtained above is centrifuged at 1000-3000 rpm for 5-30 min to remove the unpeeled hexagonal boron nitride, the supernatant is further centrifuged at 10000-20000 rpm for 30-60 min, and the obtained solid is dried at 80-100° C. for 8-12 h to obtain boron nitride nanosheets;

[0028] BN3, adding the above-mentioned boron nitride nanosheets and 3-thiocyanatopropyltriethoxysilane into acetone, stirring and reacting at 40-80°C at a speed of 300-1000rpm for 12-24h, wherein the mass of 3-thiocyanatopropyltriethoxysilane is 1%-5% of the boron nitride nanosheets, and the mass of acetone is 50-200 times that of the boron nitride nanosheets;

[0029] BN4, centrifuge to remove the solvent and unreacted silane coupling agent, wash with ethanol 3 to 5 times, and then dry in an oven at 60 to 100° C. for 8 to 24 hours to obtain the boron nitride thiocyanate.

[0030] It should be noted that the thermal conductivity of the self-healing silicone thermally conductive gel prepared by the method of the present invention is greater than 2.5 W / (m·K), and the room temperature self-healing efficiency is greater than 95%, and can be applied to the heat dissipation field of electronic components.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] 1) In view of the fact that traditional thermal management materials may suffer mechanical damage under the dual effects of long-term use and internal stress, thereby weakening their thermal conductivity, and the relatively complex preparation of existing self-healing thermal management materials, the present invention proposes to use the thiocyanate groups of thiocyanated polydimethylsiloxane and thiocyanated boron nitride to form a dynamically reversible thiocyanate metal salt complex with metal salts to achieve self-healing, and at the same time, use thiocyanate boron nitride to improve the thermal conductivity to prepare a self-healing thermal conductive gel.

[0033] 2) The present invention provides a method for preparing thiocyanated polydimethylsiloxane and thiocyanated boron nitride. The thermal conductivity of the self-healing silicone thermally conductive gel prepared by the method is greater than 2.5W / (m·K), and the room temperature self-healing efficiency is greater than 95%. The preparation method of the self-healing silicone thermally conductive gel of the present invention has low requirements on equipment, is simple to operate, and can be used for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0035] Figure 1 This is the SEM image of modified BN.

[0036] Figure 2 The repair efficiency of the thermally conductive gel prepared in the examples and comparative examples. DETAILED DESCRIPTION

[0037] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] The word "embodiment" used here as an "exemplary" does not necessarily mean that any embodiment described is superior to or better than other embodiments. Unless otherwise specified, the performance index tests in the embodiments of this application are performed using conventional test methods in the art. It should be understood that the terms described in this application are only used to describe specific implementation methods and are not used to limit the content disclosed in this application.

[0039] Unless otherwise specified, the technical and scientific terms used in this document have the same meanings as commonly understood by ordinary technicians in the technical field to which this application belongs; other experimental methods and technical means not specifically specified in this application refer to experimental methods and technical means commonly used by ordinary technicians in this field.

[0040] In order to better illustrate the content of the present application, numerous specific details are provided in the specific examples below. It should be understood by those skilled in the art that the present application can also be implemented without certain specific details. In the embodiments, some methods, means, instruments, equipment, etc. well known to those skilled in the art are not described in detail in order to highlight the main purpose of the present application.

[0041] Under the premise of no conflict, the technical features disclosed in the embodiments of the present application can be combined arbitrarily, and the resulting technical solutions belong to the contents disclosed in the embodiments of the present application.

[0042] The invention discloses a self-repairing organic silicon thermal conductive gel and a preparation method thereof.

[0043] In order to better understand the present invention, the present invention is further specifically described below through the following examples, but it should not be understood as a limitation of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above invention content are also considered to fall within the protection scope of the present invention.

[0044] Example 1

[0045] Preparation of polydimethylsiloxane thiocyanate:

[0046] P1. Place polydimethylsiloxane with a viscosity of 8000 mPa·s in a plasma cleaning device, select oxygen as the process gas, adjust the pressure to 100 Pa, and treat for 15 seconds to obtain hydroxylated polydimethylsiloxane;

[0047] P2. Add 10 g of the above hydroxylated polydimethylsiloxane and 0.1 g of 3-thiocyanatopropyltriethoxysilane into 500 g of acetone, and stir at 500 rpm at 60° C. to react for 12 h;

[0048] P3. Remove the solvent by rotary evaporation at 60°C to obtain thiocyanate polydimethylsiloxane.

[0049] Preparation of Boron Nitride Thiocyanate:

[0050] BN1, 5g of hexagonal boron nitride powder was dispersed in a mixed solution of 50g of isopropanol and 50g of deionized water, and ultrasonically stripped at 300W for 24h;

[0051] BN2, the dispersion obtained above was centrifuged at 2000 rpm for 10 min to remove the unpeeled hexagonal boron nitride, the supernatant was further centrifuged at 10000 rpm for 30 min, and the obtained solid was dried at 80 ° C for 12 h to obtain boron nitride nanosheets;

[0052] BN3, add 1g of the above-mentioned boron nitride nanosheets and 0.02g of 3-thiocyanatopropyltriethoxysilane into 100g of acetone, and stir at 500rpm at 60°C for 12h;

[0053] BN4, centrifuge to remove the solvent and unreacted silane coupling agent, wash with ethanol three times, and then dry in an oven at 60°C for 24 hours to obtain boron nitride thiocyanate.

[0054] Preparation of self-healing silicone thermally conductive gel:

[0055] 100 parts of thiocyanate polydimethylsiloxane, 30 parts of thiocyanate boron nitride and 5 parts of cupric chloride were mixed in a planetary mixer for 10 minutes, and then vacuum degassed until there were no bubbles. The mixture was poured into a polytetrafluoroethylene mold and placed in a vacuum drying oven to react at 80°C for 2 hours, and then at 120°C for 4 hours to obtain a self-healing silicone thermal conductive gel.

[0056] The thermal conductivity of the prepared self-healing silicone thermally conductive gel is 2.52 W / (m·K), and the room temperature repair efficiency is 96.3%.

[0057] Example 2

[0058] Preparation of thiocyanate polydimethylsiloxane: the same as in Example 1.

[0059] Preparation of boron nitride thiocyanate: the same as in Example 1.

[0060] Preparation of self-healing silicone thermally conductive gel:

[0061] 100 parts of thiocyanate polydimethylsiloxane, 40 parts of thiocyanate boron nitride and 6 parts of cupric chloride were mixed in a planetary mixer for 10 minutes, and then vacuum degassed until there were no bubbles. The mixture was poured into a polytetrafluoroethylene mold and placed in a vacuum drying oven to react at 80°C for 2 hours, and then at 120°C for 4 hours to obtain a self-healing silicone thermal conductive gel.

[0062] The thermal conductivity of the prepared self-healing silicone thermally conductive gel is 2.70 W / (m·K), and the room temperature repair efficiency is 96.9%.

[0063] Example 3

[0064] Preparation of thiocyanate polydimethylsiloxane: the same as in Example 1.

[0065] Preparation of boron nitride thiocyanate: the same as in Example 1.

[0066] Preparation of self-healing silicone thermally conductive gel:

[0067] 100 parts of thiocyanate polydimethylsiloxane, 50 parts of thiocyanate boron nitride and 7 parts of zinc chloride were mixed in a planetary mixer for 10 minutes, and then vacuum degassed until there were no bubbles. The mixture was poured into a polytetrafluoroethylene mold and placed in a vacuum drying oven to react at 80°C for 2 hours, and then at 120°C for 4 hours to obtain a self-healing silicone thermal conductive gel.

[0068] The thermal conductivity of the prepared self-healing silicone thermally conductive gel is 2.98 W / (m·K), and the room temperature repair efficiency is 97.4%.

[0069] Example 4

[0070] Preparation of thiocyanate polydimethylsiloxane: the same as in Example 1.

[0071] Preparation of boron nitride thiocyanate: the same as in Example 1.

[0072] Preparation of self-healing silicone thermally conductive gel:

[0073] 100 parts of polydimethylsiloxane thiocyanate, 70 parts of boron nitride thiocyanate and 9 parts of nickel nitrate were mixed in a planetary mixer for 20 minutes, and then vacuum degassed until there were no bubbles. The mixture was poured into a polytetrafluoroethylene mold and placed in a vacuum drying oven to react at 80°C for 2 hours, and then at 120°C for 4 hours to obtain a self-healing silicone thermal conductive gel.

[0074] The thermal conductivity of the prepared self-healing silicone thermally conductive gel is 3.85 W / (m·K), and the room temperature repair efficiency is 98.2%.

[0075] Example 5

[0076] Preparation of polydimethylsiloxane thiocyanate:

[0077] P1. Place polydimethylsiloxane with a viscosity of 8000 mPa·s in a plasma cleaning device, select oxygen as the process gas, adjust the pressure range to 100 Pa, and after 30 seconds of treatment, obtain hydroxylated polydimethylsiloxane;

[0078] P2. Add 10 g of the above hydroxylated polydimethylsiloxane and 0.2 g of 3-thiocyanatopropyltriethoxysilane into 500 g of acetone, and stir at 500 rpm at 60° C. to react for 12 h;

[0079] P3. Remove the solvent by rotary evaporation at 60°C to obtain thiocyanate polydimethylsiloxane.

[0080] Preparation of boron nitride thiocyanate: the same as in Example 1.

[0081] Preparation of self-healing silicone thermally conductive gel:

[0082] 100 parts of thiocyanate polydimethylsiloxane, 30 parts of thiocyanate boron nitride and 5 parts of cupric chloride were mixed in a planetary mixer for 10 minutes, and then vacuum degassed until there were no bubbles. The mixture was poured into a polytetrafluoroethylene mold and placed in a vacuum drying oven to react at 80°C for 2 hours, and then at 120°C for 4 hours to obtain a self-healing silicone thermal conductive gel.

[0083] The thermal conductivity of the prepared self-healing silicone thermally conductive gel is 2.55 W / (m·K), and the room temperature repair efficiency is 96.7%.

[0084] Example 6

[0085] Preparation of thiocyanate polydimethylsiloxane: the same as in Example 5.

[0086] Preparation of boron nitride thiocyanate: the same as in Example 1.

[0087] Preparation of self-healing silicone thermally conductive gel:

[0088] 100 parts of polydimethylsiloxane thiocyanate, 70 parts of boron nitride thiocyanate and 9 parts of nickel nitrate were mixed in a planetary mixer for 10 minutes, and then vacuum degassed until there were no bubbles. The mixture was poured into a polytetrafluoroethylene mold and placed in a vacuum drying oven to react at 80°C for 2 hours, and then at 120°C for 4 hours to obtain a self-healing silicone thermal conductive gel.

[0089] The thermal conductivity of the prepared self-healing silicone thermally conductive gel is 3.88 W / (m·K), and the room temperature repair efficiency is 98.5%.

[0090] Example 7

[0091] Preparation of thiocyanate polydimethylsiloxane: the same as in Example 1.

[0092] Preparation of Boron Nitride Thiocyanate:

[0093] BN1, 5g of hexagonal boron nitride powder was dispersed in a mixed solution of 50g of isopropanol and 50g of deionized water, and ultrasonically stripped at 300W for 24h;

[0094] BN2, the dispersion obtained above was centrifuged at 2000 rpm for 10 min to remove the unpeeled hexagonal boron nitride, the supernatant was further centrifuged at 10000 rpm for 30 min, and the obtained solid was dried at 80 ° C for 12 h to obtain boron nitride nanosheets;

[0095] BN3, add 1g of the above-mentioned boron nitride nanosheets and 0.03g of 3-thiocyanatopropyltriethoxysilane into 100g of acetone, and stir at 500rpm at 60°C for 12h;

[0096] BN4, centrifuge to remove the solvent and unreacted silane coupling agent, wash with ethanol three times, and then dry in an oven at 60°C for 24 hours to obtain boron nitride thiocyanate.

[0097] Preparation of self-healing silicone thermally conductive gel:

[0098] 100 parts of thiocyanate polydimethylsiloxane, 30 parts of thiocyanate boron nitride and 5 parts of cupric chloride were mixed in a planetary mixer for 10 minutes, and then vacuum degassed until there were no bubbles. The mixture was poured into a polytetrafluoroethylene mold and placed in a vacuum drying oven to react at 80°C for 2 hours, and then at 120°C for 4 hours to obtain a self-healing silicone thermal conductive gel.

[0099] The thermal conductivity of the prepared self-healing silicone thermally conductive gel is 2.58 W / (m·K), and the room temperature repair efficiency is 97.3%.

[0100] Example 8

[0101] Preparation of thiocyanate polydimethylsiloxane: the same as in Example 1.

[0102] Preparation of boron nitride thiocyanate: consistent with Example 7.

[0103] Preparation of self-healing silicone thermally conductive gel:

[0104] 100 parts of polydimethylsiloxane thiocyanate, 70 parts of boron nitride thiocyanate and 9 parts of nickel nitrate were mixed in a planetary mixer for 10 minutes, and then vacuum degassed until there were no bubbles. The mixture was poured into a polytetrafluoroethylene mold and placed in a vacuum drying oven to react at 80°C for 2 hours, and then at 120°C for 4 hours to obtain a self-healing silicone thermal conductive gel.

[0105] The thermal conductivity of the prepared self-healing silicone thermally conductive gel is 3.92 W / (m·K), and the room temperature repair efficiency is 99.0%.

[0106] Example 9

[0107] Preparation of thiocyanate polydimethylsiloxane: the same as in Example 5.

[0108] Preparation of boron nitride thiocyanate: consistent with Example 7.

[0109] Preparation of self-healing silicone thermally conductive gel:

[0110] 100 parts of thiocyanate polydimethylsiloxane, 30 parts of thiocyanate boron nitride and 5 parts of cupric chloride were mixed in a planetary mixer for 10 minutes, and then vacuum degassed until there were no bubbles. The mixture was poured into a polytetrafluoroethylene mold and placed in a vacuum drying oven to react at 80°C for 2 hours, and then at 120°C for 4 hours to obtain a self-healing silicone thermal conductive gel.

[0111] The thermal conductivity of the prepared self-healing silicone thermally conductive gel is 2.60 W / (m·K), and the room temperature repair efficiency is 97.5%.

[0112] Example 10

[0113] Preparation of thiocyanate polydimethylsiloxane: the same as in Example 5.

[0114] Preparation of boron nitride thiocyanate: consistent with Example 7.

[0115] Preparation of self-healing silicone thermally conductive gel:

[0116] 100 parts of polydimethylsiloxane thiocyanate, 70 parts of boron nitride thiocyanate and 9 parts of nickel nitrate were mixed in a planetary mixer for 10 minutes, and then vacuum degassed until there were no bubbles. The mixture was poured into a polytetrafluoroethylene mold and placed in a vacuum drying oven to react at 80°C for 2 hours, and then at 120°C for 4 hours to obtain a self-healing silicone thermal conductive gel.

[0117] The thermal conductivity of the prepared self-healing silicone thermally conductive gel is 3.94 W / (m·K), and the room temperature repair efficiency is 99.3%.

[0118] In order to further demonstrate the beneficial effects of the present invention and to better understand the present invention, the following comparative examples are used to further illustrate the technical features disclosed in the present invention, but they should not be construed as limiting the present invention. Other improvements made by those skilled in the art based on the above invention content without inventive work are also considered to fall within the scope of protection of the present invention.

[0119] Comparative Example 1

[0120] Preparation of amino polydimethylsiloxane:

[0121] P1. Place polydimethylsiloxane with a viscosity of 8000 mPa·s in a plasma cleaning device, select oxygen as the process gas, adjust the pressure range to 100 Pa, and obtain hydroxylated polydimethylsiloxane after 15 seconds of treatment;

[0122] P2. Add 10 g of the above hydroxylated polydimethylsiloxane and 0.1 g of 3-aminopropyltriethoxysilane into 500 g of acetone, and stir at 60° C. and 500 rpm for 12 h.

[0123] P3. Remove the solvent by rotary evaporation at 60°C to obtain amino polydimethylsiloxane.

[0124] Preparation of boron nitride thiocyanate: the same as in Example 1.

[0125] Preparation of self-healing silicone thermally conductive gel:

[0126] 100 parts of amino polydimethylsiloxane, 30 parts of boron nitride thiocyanate and 5 parts of cupric chloride were mixed in a planetary mixer for 10 minutes, and then vacuum degassed until there were no bubbles. The mixture was poured into a polytetrafluoroethylene mold and placed in a vacuum drying oven to react at 80°C for 2 hours, and then at 120°C for 4 hours to obtain a self-healing silicone thermal conductive gel.

[0127] The thermal conductivity of the prepared self-healing silicone thermally conductive gel is 2.46 W / (m·K), and the room temperature repair efficiency is 67.3%.

[0128] Comparative Example 2

[0129] Preparation of thiocyanate polydimethylsiloxane: the same as in Example 1.

[0130] Preparation of amination boron nitride:

[0131] BN1, 5g of hexagonal boron nitride powder was dispersed in a mixed solution of 50g of isopropanol and 50g of deionized water, and ultrasonically stripped at 300W for 24h;

[0132] BN2, the dispersion obtained above was centrifuged at 2000 rpm for 10 min to remove the unpeeled hexagonal boron nitride, the supernatant was further centrifuged at 10000 rpm for 30 min, and the obtained solid was dried at 80 ° C for 12 h to obtain boron nitride nanosheets;

[0133] BN3, add 1g of the above-mentioned boron nitride nanosheets and 0.02g of 3-aminopropyltriethoxysilane into 100g of acetone, and stir at 500rpm at 60°C for 12h;

[0134] BN4, centrifuge to remove the solvent and unreacted silane coupling agent, wash with ethanol three times, and then dry in an oven at 60°C for 24 hours to obtain amino boron nitride.

[0135] Preparation of self-healing silicone thermally conductive gel:

[0136] 100 parts of thiocyanate polydimethylsiloxane, 30 parts of aminated boron nitride and 5 parts of cupric chloride were mixed in a planetary mixer for 10 minutes, and then vacuum degassed until there were no bubbles. The mixture was poured into a polytetrafluoroethylene mold and placed in a vacuum drying oven to react at 80°C for 2 hours, and then at 120°C for 4 hours to obtain a self-healing silicone thermal conductive gel.

[0137] The thermal conductivity of the prepared self-healing silicone thermally conductive gel is 2.42 W / (m·K), and the room temperature repair efficiency is 83.5%.

[0138] Comparative Example 3

[0139] Preparation of amino polydimethylsiloxane: the same as that of Comparative Example 1.

[0140] Preparation of amino boron nitride: the same as that of Comparative Example 2.

[0141] Preparation of silicone thermally conductive gel:

[0142] 100 parts of amino polydimethylsiloxane, 30 parts of amino boron nitride and 5 parts of cupric chloride were mixed in a planetary mixer for 10 minutes, and then vacuum degassed until there were no bubbles. The mixture was poured into a polytetrafluoroethylene mold and placed in a vacuum drying oven to react at 80°C for 2 hours, and then at 120°C for 4 hours to obtain a silicone thermal conductive gel.

[0143] The thermal conductivity of the prepared organic silicon thermally conductive gel is 2.52 W / (m·K), and the room temperature repair efficiency is 0%.

[0144] In addition, in order to further illustrate / verify the superiority of the technology of the present invention, the inventors also conducted the following performance tests:

[0145] The thermal conductivity and repair efficiency of the silicone thermally conductive gels prepared in Examples 1-10 and Comparative Examples 1-2 were tested respectively. The results are shown in Table 1.

[0146] Table 1 Thermal conductivity and repair efficiency of thermally conductive gel in Examples 1-10 and Comparative Examples 1-2

[0147] Thermally conductive gel Thermal conductivity (W / m·K) Repair efficiency Example 1 2.52 96.3 Example 2 2.70 96.9 Example 3 2.98 97.4 Example 4 3.85 98.2 Example 5 2.55 96.7 Example 6 3.88 98.5 Example 7 2.58 97.3 Example 8 3.92 99.0 Example 9 2.60 97.5 Example 10 3.94 99.3 Comparative Example 1 2.46 67.3 Comparative Example 2 2.42 83.5 Comparative Example 3 2.52 0

[0148] It can be seen from Table 1 that in Comparative Examples 1-3, when only one of polydimethylsiloxane or boron nitride or neither of them is subjected to thiocyanate modification, the thermal conductivity and repair efficiency of the obtained silicone thermally conductive gel are significantly reduced, indicating that after thiocyanate modification, a reversible thiocyanate metal salt complex can be formed with a metal salt to achieve self-repair.

[0149] The above experiments show that the thermal conductivity of the self-healing silicone thermally conductive gel prepared by the present invention is greater than 2.5W / (m·K) and the repair efficiency is greater than 96%. In addition, the preparation method of the present invention has low requirements on equipment and is simple to operate, and can be used for large-scale production.

[0150] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A self-repairing silicone thermally conductive gel, characterized in that: The self-repairing silicone thermally conductive gel comprises the following components in parts by weight: 50-100 parts of thiocyanate polydimethylsiloxane, 30-80 parts of thiocyanate boron nitride, and 5-20 parts of metal salt; The thiocyanate group of the thiocyanate polydimethylsiloxane can form a thiocyanate metal salt complex with a metal salt; The thiocyanate group of the thiocyanated boron nitride can form a thiocyanate metal salt complex with a metal salt.

2. The self-repairing silicone thermally conductive gel according to claim 1, characterized in that: The structural formula of the polydimethylsiloxane thiocyanate is shown in Formula I:

3. The self-repairing silicone thermally conductive gel according to claim 1, characterized in that: The structural formula of the boron nitride thiocyanate is shown in Formula II:

4. The self-repairing silicone thermally conductive gel according to claim 1, characterized in that: The metal salt is one or more combinations of copper chloride, copper sulfate, copper nitrate, zinc chloride, zinc sulfate, zinc nitrate, nickel chloride, nickel sulfate, nickel nitrate, ferric chloride, ferric sulfate, ferric nitrate, manganese chloride, manganese sulfate, and manganese nitrate.

5. A method for preparing the self-repairing silicone thermally conductive gel according to claim 1, characterized in that: The method specifically comprises the following steps: The polydimethylsiloxane thiocyanate, boron nitride thiocyanate and metal salt are mixed in a planetary mixer for 5 to 60 minutes, and then vacuum degassing is performed until there are no bubbles, poured into a polytetrafluoroethylene mold, placed in a vacuum drying oven at 80 to 100° C. for reaction for 1 to 2 hours, and then at 100 to 120° C. for reaction for 2 to 4 hours to obtain the self-healing silicone thermal conductive gel.

6. The method for preparing the self-repairing silicone thermally conductive gel according to claim 5, characterized in that: The thiocyanate polydimethylsiloxane is obtained by first subjecting polydimethylsiloxane to plasma treatment and then to modification with 3-thiocyanatepropyltriethoxysilane; the thiocyanate boron nitride is obtained by dispersing and exfoliating hexagonal boron nitride to obtain boron nitride nanosheets, and then the boron nitride nanosheets are modified with 3-thiocyanatepropyltriethoxysilane.

7. The method for preparing the self-repairing silicone thermally conductive gel according to claim 5, characterized in that: The preparation steps of the thiocyanate polydimethylsiloxane are as follows: P1. Placing polydimethylsiloxane in a plasma cleaning device, selecting oxygen as a process gas, adjusting the pressure to 25 to 135 Pa, and treating for 15 to 60 seconds to obtain hydroxylated polydimethylsiloxane, wherein the viscosity of the polydimethylsiloxane at 25° C. is 5000 to 20000 mPa·s; P2. Add the hydroxylated polydimethylsiloxane prepared in P1 and 3-thiocyanatopropyltriethoxysilane to acetone, and stir the mixture at 40-80°C at a speed of 300-1000 rpm for 12-24 hours, wherein the mass of 3-thiocyanatopropyltriethoxysilane is 1%-5% of the hydroxylated polydimethylsiloxane, and the mass of acetone is 50-200 times that of the hydroxylated polydimethylsiloxane; after the reaction is completed, remove the solvent by rotary evaporation at 40-80°C to obtain the thiocyanato polydimethylsiloxane.

8. The method for preparing the self-repairing silicone thermally conductive gel according to claim 5, characterized in that: The preparation steps of the thiocyanate boron nitride are as follows: BN1, dispersing hexagonal boron nitride powder in a mixed solution of isopropanol and deionized water, and ultrasonically exfoliating for 12 to 24 hours under 100 to 500W ultrasound, wherein the volume ratio of isopropanol to deionized water is 1:1, and the mass ratio of hexagonal boron nitride powder to deionized water is 0.05 to 0.2; BN2, the dispersion obtained in step BN1 is centrifuged at 1000-3000 rpm for 5-30 min to remove the unpeeled hexagonal boron nitride, the supernatant is further centrifuged at 10000-20000 rpm for 30-60 min, and the obtained solid is dried at 80-100° C. for 8-12 h to obtain boron nitride nanosheets; BN3, adding the boron nitride nanosheets and 3-thiocyanatopropyltriethoxysilane obtained in step BN2 to acetone, stirring and reacting at 40-80°C at a speed of 300-1000rpm for 12-24h, wherein the mass of 3-thiocyanatopropyltriethoxysilane is 1%-5% of the boron nitride nanosheets, and the mass of acetone is 50-200 times that of the boron nitride nanosheets; BN4, centrifuge to remove the solvent and unreacted silane coupling agent, wash with ethanol 3 to 5 times, and then dry in an oven at 60 to 100° C. for 8 to 24 hours to obtain the boron nitride thiocyanate.

Citation Information

Cited By

  • Repairable liquid crystal type organic silicon heat conduction material as well as preparation method and application thereof

    CN120271828A