Novel heat storage material as well as preparation method and application thereof
By using new heat storage materials with high temperature resistant shells and metal alloy cores in the dehydrogenation reaction, the problem of low heat storage efficiency of heat storage materials in the prior art is solved, and the catalyst is significantly improved The heat storage and release efficiency of the bed improves the space utilization and production capacity of the reactor.
Patent Information
- Application Number
- CN202310780685.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-28
- Publication Date
- 2024-12-31
AI Technical Summary
The existing heat storage materials have low heat storage efficiency in the dehydrogenation reaction, resulting in uneven temperature distribution of the catalyst bed, affecting conversion and selectivity, and low equipment space utilization, so the equipment size needs to be increased to improve production capacity.
Using a new heat storage material composed of a high-temperature resistant shell and metal alloy core, it is prepared by thermal spraying technology. The phase-change heat of the metal alloy core achieves efficient heat storage, combined with SiO2 sol impregnation to improve surface smoothness and improve heat storage and release efficiency. .
It significantly improves the heat storage capacity of the heat storage material, increases the volume ratio of the catalyst actually used for the dehydrogenation reaction in the catalyst bed, thereby improving the space utilization rate of the alkane dehydrogenation reactor, reducing the equipment size, and improving the Production capacity.
Smart Images

Figure CN119220226A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical materials, and specifically relates to a new type of heat storage material and a preparation method and application thereof. Background Art
[0002] Thermal storage materials are common thermal storage components in thermal storage equipment, usually including metal thermal storage materials, ceramic thermal storage materials and phase change thermal storage materials. The dehydrogenation reaction absorbs a lot of heat, causing the catalyst bed temperature to drop, and the carbon deposits generated by the reaction will also cause the catalyst activity to drop rapidly. Therefore, in order to ensure that the catalyst activity is within the optimal range, it is necessary to regenerate once every period of time and heat the catalyst bed again to accumulate a certain amount of heat to prepare for the next reaction. The dehydrogenation reaction is usually operated under high temperature, negative pressure or low pressure conditions, and the effect of temperature on the reaction is very significant. Excessive reaction temperature will lead to the occurrence of side reactions such as cracking, and further produce carbon deposits to reduce the activity of the catalyst, resulting in a decrease in selectivity. On the other hand, too low a reaction temperature will cause a rapid decrease in conversion. When the catalyst bed temperature is unevenly distributed, it will lead to the appearance of local hot spots or local cold spots, resulting in a decrease in conversion rate or selectivity. Therefore, the thermal storage and temperature control of the catalyst bed are very critical issues in the dehydrogenation reaction.
[0003] The commonly used heat storage material is inert alumina. Depending on the raw materials of the dehydrogenation reaction, the ratio of inert alumina to catalyst is not exactly the same. For the propane dehydrogenation process, the volume of inert alumina can account for about 50% of the volume of the entire catalyst bed; and for the isobutane dehydrogenation process, the volume of inert alumina can account for about 30% of the volume of the entire catalyst bed. Therefore, the catalyst actually used for the dehydrogenation reaction in the catalyst bed only accounts for about 50-70% of the volume of the entire catalyst bed. A large amount of reactor space is occupied by inert alumina used for heat storage, and the space utilization rate of the alkane dehydrogenation reactor is low, which affects the production capacity of the device and has to increase the size of the equipment.
[0004] In other technical reports, reports of other heat-generating materials are also disclosed. For example, CN106029612A discloses an improved endothermic dehydrogenation process of alkanes using heat-generating materials. In the process, in addition to using CATOFIN@300 catalyst and inert alumina, HGM heat-generating materials (metal elements such as copper and manganese are loaded on alumina) are also used, including reacting hydrocarbons with a multi-component catalyst bed and regenerating the catalyst bed using air, wherein the air and hydrocarbons used in the regeneration step are at a low air / hydrocarbon ratio and a pressure close to atmospheric pressure, which improves the efficiency of the process. The added heat-generating material is mainly used to provide heat to reduce the air consumption during the regeneration process, and cannot increase the heat storage capacity of the bed, and a large amount of inert alumina still needs to be added to the catalyst bed.
[0005] CN107074683A discloses a CuO thermal release material, wherein Cu and CO are formed by the reaction of CO and CuO. 2 , releasing heat. However, this method introduces CO and CO 2 Components such as the above will cause the partial pressure of the reaction gas to decrease, affecting the reaction conversion rate.
[0006] The heat sources in CN108300430B are mainly: CuO and H 2 The reaction releases heat and generates water, the heat-generating material absorbs water and releases heat, and the additive stores part of the heat as a heat medium. However, this method requires the consumption of additional hydrogen, and the generated water will accelerate the formation of α-chromium-aluminum in the catalyst, resulting in a significant decrease in the reaction conversion rate.
[0007] At present, the thermal storage materials need to be further improved and enhanced during the dehydrogenation reaction. Summary of the invention
[0008] In order to solve the above problems in the prior art, the present invention proposes a new type of thermal storage material and a preparation method and application thereof.
[0009] In a first aspect, the present invention provides a novel heat storage material, which is composed of a high temperature resistant outer shell and a metal alloy inner core.
[0010] As a specific embodiment of the present invention, the high temperature resistant shell is an inert metal oxide, preferably selected from alumina, α-alumina, γ-alumina, silicon oxide, aluminum oxide and silicon oxide; wherein the mass ratio of aluminum oxide to silicon oxide in the aluminum oxide and silicon oxide is 1:(0.6-1). The thermal conductivity of the high temperature resistant shell material is 20-35W / (m·K).
[0011] As a specific embodiment of the present invention, the metal alloy core is an aluminum alloy, preferably selected from aluminum-magnesium alloy and cast aluminum alloy; the melting point of the metal alloy core is 500-650°C, preferably 560-620°C; the phase change heat of the metal alloy core is 250-550 kJ / kg.
[0012] According to the present invention, the magnesium content in the aluminum-magnesium alloy is 0.5-5wt%, and the alloy also contains metal elements such as silicon, iron, copper, manganese, chromium, and zinc. Cast aluminum alloys include those mainly containing silicon (silicon content 8.0-12.5wt%), those mainly containing copper (copper content 4.0-7.0wt%), and those mainly containing zinc (copper content 5.5-6.5wt%). The melting point of the metal alloy core is related to the content of the above elements, which varies according to the alloy grade. As long as the melting point and phase change heat of the alloy are within the range required by the present invention, it is considered to be an alloy core material that meets the requirements of the present invention.
[0013] As a specific embodiment of the present invention, the particle size of the novel heat storage material is 3-50 mm, preferably 10-20 mm; the particle size of the metal alloy core is 2-49 mm, and the thickness of the high temperature resistant shell is 10-500 μm.
[0014] In a second aspect, the present invention provides a method for preparing the novel thermal storage material, comprising the following steps:
[0015] S1: preparing the alloy core material into small balls with a desired particle size by mechanical processing to obtain the metal alloy core;
[0016] S2: The surface of the metal alloy core obtained in step S1 is subjected to one or more thermal spraying to obtain the high temperature resistant shell and the novel heat storage material.
[0017] As a specific embodiment of the present invention, the preparation method further includes: Optionally, S3: placing the new thermal storage material prepared in step S2 into SiO 2 The purpose of step S3 is to attach a layer of silicon oxide to the aluminum oxide formed by thermal spraying, so that the particle surface is smoother and the local metal alloy core is exposed due to uneven thermal spraying.
[0018] As a specific embodiment of the present invention, in the step S1, the particle size of the metal alloy core obtained is 2 to 49 mm, preferably 10 to 20 mm.
[0019] As a specific implementation of the present invention, in step S2, the spraying thickness of the high temperature resistant shell is 10 to 500 μm.
[0020] In a third aspect, the present invention provides application of the novel thermal storage material in the field of dehydrogenation reactors.
[0021] As a specific embodiment of the present invention, the novel heat storage material is added to the catalyst bed of the dehydrogenation reactor to improve the space utilization rate of the alkane dehydrogenation reactor.
[0022] The new heat storage material provided by the present invention utilizes the phase change heat of metal alloys to achieve heat storage. Specifically, in the dehydrogenation process of low-carbon alkanes, the new heat storage material and catalyst in the reactor bed are heated to 600-650°C by regeneration air. During the regeneration process, the metal alloy core absorbs heat and melts into a liquid phase, thereby achieving a large amount of heat storage. In the dehydrogenation reaction stage, the reaction temperature is 560-620°C, and the metal alloy melted into a liquid phase releases a large amount of heat and becomes a solid phase to maintain the temperature of the catalyst bed. The metal alloy core in the new heat storage material provided by the present invention is an aluminum alloy, and its phase change heat in the melting process is 250-550 kJ / kg, while the heat capacity of inert alumina is about 0.7-0.9 kJ / kg°C. In the same dehydrogenation reaction process, the new heat storage material provided by the present invention can provide 6-10 times the heat of the same mass of inert alumina. Therefore, compared with the inert alumina heat storage material used in the prior art, the catalyst actually used for the dehydrogenation reaction in the catalyst bed only accounts for about 50-70% of the volume of the entire catalyst bed. However, by using the new heat storage material provided by the present invention, the catalyst actually used for the dehydrogenation reaction in the catalyst bed can account for 71-95% of the volume of the entire catalyst bed, and the space utilization rate of the alkane dehydrogenation reactor is increased by more than 25%.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] 1. The novel heat storage material of the present invention adopts phase change heat storage, and has a higher heat storage capacity, which is 6 to 10 times that of the inert alumina used in the prior art.
[0025] 2. The method of improving the space utilization rate of the alkane dehydrogenation reactor of the present invention has a low filling ratio of the new heat storage material, and the catalyst occupies a greatly increased bed volume, so that the space utilization rate of the alkane dehydrogenation reactor is increased by more than 25%, which can significantly reduce the size of the reactor equipment and improve the production capacity. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 A schematic diagram of a novel heat storage material provided by the present invention;
[0027] Figure 2 A schematic diagram of a catalyst bed for improving the space utilization rate of an alkane dehydrogenation reactor provided by the present invention;
[0028] Figure 3 Schematic diagram of the catalyst bed provided by the prior art.
[0029] Among them, 1-catalyst bed; 2-catalyst; 3-new heat storage material, 3a-high temperature resistant shell, 3b-metal alloy core; 4-inert alumina ceramic ball. DETAILED DESCRIPTION
[0030] The present invention will be further described below in conjunction with specific embodiments, but they do not constitute any limitation to the present invention.
[0031] The catalyst information used in each embodiment of the present invention is as follows:
[0032] Cr metal-containing catalyst: a catalyst containing Cr metal on an alumina carrier (Cr content 10 wt%);
[0033] Catalyst containing Pt metal: a catalyst containing Pt metal supported on an alumina carrier (Pt content: 0.3 wt %).
[0034] Example 1
[0035] This embodiment provides a new type of thermal storage material and a preparation method thereof, the specific details of which are as follows:
[0036] S1: preparing the alloy core material into small balls with a desired particle size by mechanical processing to obtain the metal alloy core;
[0037] S2: The surface of the metal alloy core obtained in step S1 is subjected to multiple thermal spraying to obtain the high temperature resistant shell that fully wraps the metal alloy core to obtain the novel heat storage material.
[0038] The high temperature resistant outer shell of the novel heat storage material obtained in Example 1 is made of alumina, the alloy material of the inner core is aluminum-magnesium alloy, the melting point of the metal alloy inner core is 580° C., and the particle size is 10 mm.
[0039] Embodiments 2 to 12
[0040] Embodiments 2 to 12: The new thermal storage material obtained by the preparation method provided in Embodiment 1 is observed to see whether the metal alloy core of the new thermal storage material obtained in step S2 is exposed. If so, SiO 2 The material was immersed in the sol for 1 minute, and the immersed material was dried to obtain the novel thermal storage material. As shown in Table 1:
[0041] Table 1 New thermal storage materials prepared in Examples 1 to 12
[0042]
[0043]
[0044] Embodiment 13
[0045] The new heat storage material prepared in Example 1 was added to the catalyst bed containing Cr metal, and the volume ratio of the new heat storage material to the catalyst was 0.1:1. The new heat storage material and the catalyst in the catalyst bed were uniformly mixed, such as Figure 2In the catalyst bed, the catalyst accounts for 91% of the bed volume.
[0046] The propane dehydrogenation to propylene reaction was carried out in a reactor filled with the above catalyst bed. The dehydrogenation reaction was carried out in a reaction-regeneration cycle mode, with a reaction time of 10 minutes, a nitrogen purge of 1 minute, a regeneration of 10 minutes, a nitrogen purge of 1 minute, and an evacuation of 1 minute. The reaction temperature was 600°C, the pressure was 50 kPa absolute, and the propane space velocity was 0.6 hr -1 , regeneration air temperature 650° C. The reaction results were propane conversion 47.2% and propylene selectivity 90.8%.
[0047] Embodiment 14
[0048] The novel heat storage material prepared in Example 3 was added to the catalyst bed containing Cr metal, and the volume ratio of the novel heat storage material to the catalyst was 0.05:1. The novel heat storage material and the catalyst were uniformly mixed in the catalyst bed. In the catalyst bed, the catalyst accounted for 95% of the volume of the bed.
[0049] The reaction of propane dehydrogenation to propylene was carried out in a reactor filled with the above catalyst bed. The dehydrogenation reaction was carried out in a reaction-regeneration cycle mode, with a reaction time of 10 minutes, a nitrogen purge of 1 minute, a regeneration of 10 minutes, a nitrogen purge of 1 minute, and an evacuation of 1 minute. The reaction temperature was 600°C, the pressure was 80 kPa absolute pressure, and the propane space velocity was 0.4 hr -1 , regeneration air temperature 600° C. The reaction results were propane conversion 46.4% and propylene selectivity 92.2%.
[0050] Embodiment 15
[0051] The novel heat storage material prepared in Example 10 was added to the catalyst bed containing Pt metal, and the volume ratio of the novel heat storage material to the catalyst was 0.2:1. The novel heat storage material and the catalyst were uniformly mixed in the catalyst bed. The catalyst accounted for 83% of the volume of the bed.
[0052] Five reactors loaded with the above catalyst beds were used to dehydrogenate propane to produce propylene. The reactors were alternately operated according to the process of reaction, purging, regeneration, evacuation, and reduction, wherein the reaction time was 10 minutes, purging time was 1 minute, regeneration time was 10 minutes, evacuation time was 1 minute, and reduction time was 2 minutes. The reaction temperature was 620°C, the pressure was 40 kPa absolute pressure, and the propane space velocity was 1.2 hr -1 , regeneration air temperature 660° C. The reaction results were propane conversion 51.2% and propylene selectivity 91.8%.
[0053] Comparative Example 1
[0054] In the catalyst bed containing Cr metal, a portion of inert Al 2 O3 Ceramic ball, inert Al 2 O 3 The volume ratio of ceramic balls to catalyst is 1:1, and the catalyst bed is as follows Figure 3 As shown. Inert Al 2 O 3 The ceramic balls and the catalyst are uniformly mixed. In the catalyst bed, the proportion of the catalyst in the bed volume is 50%, which is much lower than the level of the embodiment.
[0055] The propane dehydrogenation to propylene reaction was carried out in a reactor filled with the above catalyst bed. The dehydrogenation reaction was carried out in a reaction-regeneration cycle mode, with a reaction time of 10 minutes, a nitrogen purge of 1 minute, a regeneration of 10 minutes, a nitrogen purge of 1 minute, and an evacuation of 1 minute. The reaction temperature was 600°C, the pressure was 50 kPa absolute, and the propane space velocity was 0.6 hr -1 , regeneration air temperature 650° C. The reaction results were propane conversion 45.2% and propylene selectivity 88.6%.
[0056] Table 2 Summary of main conditions
[0057] Reaction conditions Embodiment 13 Embodiment 14 Embodiment 15 Comparative Example 1 New thermal storage material / catalyst volume ratio 0.1:1 0.05:1 0.2:1 - <![CDATA[Inert Al 2 O 3 Ceramic ball / catalyst volume ratio]]> - - - 1:1 Housing Material Alumina Alumina Alumina / Silicon Oxide - Alloy Material Aluminum-magnesium alloy Aluminum-magnesium alloy Aluminum-magnesium alloy - Alloy melting point / ℃ 580 580 600 - New thermal storage material particle size 10 6 40 - catalyst Cr Cr Pt Cr
[0058] Table 3 Summary of reaction results
[0059] Reaction results Embodiment 13 Embodiment 14 Embodiment 15 Comparative Example 1 Catalyst volume ratio in bed % 91 95 83 50 Dehydrogenation raw materials Propane Propane Propane Propane Conversion Rate % 47.2 46.4 51.2 45.2 Selectivity% 90.8 92.2 91.8 88.6
[0060] It can be seen from the data in Table 3 that, compared with the reaction results shown in Comparative Example 1, the method for improving the space utilization of an alkane dehydrogenation reactor provided by the present invention has a significantly higher catalyst-to-bed volume ratio, and better reaction conversion and selectivity results.
[0061] Any numerical value mentioned in the present invention, if there is only an interval of two units between any minimum value and any maximum value, includes all values from the minimum value to the maximum value each time increasing by one unit. For example, if the amount of a component, or the value of a process variable such as temperature, pressure, time, etc. is declared to be 50-90, in this specification it means that 51-89, 52-88... and 69-71 and 70-71 are specifically listed. For non-integer values, 0.1, 0.01, 0.001 or 0.0001 can be appropriately considered as a unit. These are just some specially specified examples. In this application, in a similar manner, all possible combinations of numerical values between the listed minimum and maximum values are considered to have been disclosed.
[0062] It should be noted that the embodiments described above are only used to explain the present invention and do not constitute any limitation to the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present invention may be modified as specified within the scope of the claims of the present invention, and the present invention may be revised without departing from the scope and spirit of the present invention. Although the present invention described therein relates to specific methods, materials and embodiments, it does not mean that the present invention is limited to the specific examples disclosed therein, on the contrary, the present invention can be extended to all other methods and applications with the same functions.
Claims
1. A new type of heat storage material, characterized in that: The material includes a high temperature resistant outer shell and a metal alloy core.
2. The novel heat storage material according to claim 1, characterized in that: The high temperature resistant shell is an inert metal oxide, preferably selected from alumina, α-alumina, γ-alumina, silica, alumina and silica; and / or the thermal conductivity of the high temperature resistant shell material is 20 to 35 W / (m·K).
3. The novel heat storage material according to claim 1 or 2, characterized in that: The metal alloy core is an aluminum alloy, preferably selected from aluminum-magnesium alloy and cast aluminum alloy; and / or the melting point of the metal alloy core is 500-650°C, preferably 560-620°C; and / or the phase change heat of the metal alloy core is 250-550 kJ / kg.
4. The novel heat storage material according to any one of claims 1 to 3, characterized in that: The particle size of the novel heat storage material is 3 to 50 mm, preferably 10 to 20 mm; And / or the particle size of the metal alloy core is 2-49 mm, preferably 9-19 mm; the thickness of the high temperature resistant shell is 10-500 μm, preferably 50-200 mm.
5. The method for preparing the novel thermal storage material according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1: preparing the alloy core material into small balls by mechanical processing to obtain the metal alloy core; S2: The surface of the metal alloy core obtained in step S1 is subjected to one or more thermal spraying to form a high temperature resistant shell to obtain the novel heat storage material.
6. The preparation method according to claim 5, characterized in that: The preparation method also includes: Optionally, S3: the novel heat storage material prepared in step S2 is immersed in SiO2 sol and then dried.
7. The preparation method according to claim 5 or 6, characterized in that: In the step S1, the particle size of the metal alloy core obtained is 2 to 49 mm, preferably 10 to 20 mm.
8. The preparation method according to any one of claims 5 to 7, characterized in that: In the step S2, the spraying thickness of the high temperature resistant shell is 10 to 500 μm.
9. Use of the novel heat storage material according to claims 1 to 4 or the novel heat storage material obtained by the preparation method according to any one of claims 5 to 8 in the field of dehydrogenation reactors.
10. The use according to claim 9, characterized in that: The novel heat storage material is added into the catalyst bed of the dehydrogenation reactor to improve the space utilization rate of the alkane dehydrogenation reactor.