A high specific surface area, composite ceramic technology, applied in the field of composite materials, can solve the problems of complicated preparation process, low strength, high energy consumption, etc., and achieve the effects of high specific surface area, developed mesopores, and strong adsorption capacity
Patent Information
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Publication Date
- 2017-05-10
- Estimated Expiration
- Not applicable · inactive patent
Abstract
Description
technical field
[0001] The invention relates to the technical field of composite materials, in particular to a high specific surface area composite ceramic material. Background technique
[0002] High specific surface area ceramics (also known as porous ceramics) are ceramic materials with a large number of penetrating and non-penetrating three-dimensional porous structures. , corrosion resistance, wear resistance, good biocompatibility, high specific strength, etc.) and pore characteristics (such as: low density, good thermal insulation, high specific surface area, low dielectric constant, good permeability, etc.) are effectively combined. At present, ceramics with high specific surface area have been widely used as filter materials, thermal insulation materials, artificial bone materials, electrode materials and catalyst carriers in many fields such as purification and filtration, aerospace, biomedicine, electronic devices, energy and chemical industry. Traditional high s...
Examples
Embodiment 1
[0015] A high specific surface area composite ceramic material, in parts by weight, the raw materials are: 4 parts of carbon fiber, 20 parts of ceramic particles, 2 parts of diisopropyl ether, 0.5 parts of barium hydroxide powder, 2 parts of diatomaceous earth powder, sodium carbonate powder 2 servings.
[0016] A preparation method of a high specific surface area composite ceramic material, the specific steps are:
[0017] (1) First, mix the ceramic particles, barium hydroxide powder, diatomaceous earth powder and sodium carbonate powder, then put them into the reaction kettle, carry out the melting reaction under 10MPa pressure and nitrogen protection, and obtain the mixture after cooling;
[0018] (2) Then, mix the mixture with carbon fiber and diisopropyl ether, and use ultrasonic vibration treatment under anhydrous conditions. The power of ultrasonic vibration treatment is 400W, the time is 4.5h, and it is dried at 4°C to obtain a high specific Surface area composite cer...
Embodiment 2
[0021] A high specific surface area composite ceramic material, in parts by weight, the raw materials are: 5 parts of carbon fiber, 23 parts of ceramic particles, 2 parts of diisopropyl ether, 0.7 parts of barium hydroxide powder, 2 parts of diatomite powder, barium hydroxide Magnesium powder 2 parts.
[0022] A preparation method of a high specific surface area composite ceramic material, the specific steps are:
[0023] (1) First, mix the ceramic particles, barium hydroxide powder, diatomaceous earth powder and sodium carbonate powder, then put them into the reaction kettle, carry out the melting reaction under 10MPa pressure and nitrogen protection, and obtain the mixture after cooling;
[0024] (2) Then, mix the mixture with carbon fiber and diisopropyl ether, and use ultrasonic vibration treatment under anhydrous conditions. The power of ultrasonic vibration treatment is 400W, the time is 4.5h, and it is dried at 4°C to obtain a high specific Surface area composite ceram...
Embodiment 3
[0027] A high specific surface area composite ceramic material, in parts by weight, the raw materials are: 7 parts of carbon fiber, 25 parts of ceramic particles, 3 parts of diisopropyl ether, 0.9 parts of barium hydroxide powder, 3 parts of diatomaceous earth powder, sodium carbonate powder 4 parts.
[0028] A preparation method of a high specific surface area composite ceramic material, the specific steps are:
[0029] (1) First, mix the ceramic particles, barium hydroxide powder, diatomaceous earth powder and sodium carbonate powder, then put them into the reaction kettle, carry out the melting reaction under 10MPa pressure and nitrogen protection, and obtain the mixture after cooling;
[0030] (2) Then, mix the mixture with carbon fiber and diisopropyl ether, and use ultrasonic vibration treatment under anhydrous conditions. The power of ultrasonic vibration treatment is 400W, the time is 4.5h, and it is dried at 4°C to obtain a high specific Surface area composite cerami...