Composite material for recycling waste heat of flue gas of aluminum electrolysis cell and preparation method of composite material

A composite material and flue gas waste heat technology, which is applied in the field of aluminum electrolysis waste heat recovery, can solve the problems of deteriorating production environment, reducing energy utilization rate, and reducing waste heat recovery efficiency, so as to improve corrosion resistance, reduce defects, and improve thermal shock resistance sexual effect

CN107986799AActive Publication Date: 2018-05-04CENT SOUTH UNIV
5 Cites 1 Cited by

Patent Information

Authority / Receiving Office
CN · China
Current Assignee / Owner
Publication Date
2018-05-04

Smart Images

  • Figure 1
    Figure 1
  • Figure 2
    Figure 2
  • Figure 3
    Figure 3
Patent Text Reader

Abstract

The invention discloses a composite material for recycling waste heat of flue gas of an aluminum electrolysis cell and a preparation method of the composite material. The composite material contains the following constitution raw materials in percentage by weight: 35%-45% of spinel oxide, 35%-45% of metal fibers or alloy fibers, 5%-15% of non-spinel oxide, 3%-10% of carbide, 2%-8% of nitride and 1%-5% of boride. The preparation method comprises the following steps: adding the raw materials into a ball mill, mixing, adding a ball milling medium and a bonder, and further carrying out ball milling, and drying, so as to obtain precursor powder; and putting the precursor powder into a resistance furnace, sintering at 1100-1300 DEG C for 3-9 hours in an inert atmosphere, and carrying out annealing at 300-600 DEG C for 0.5-2 hours in an oxygen atmosphere with an oxygen partial pressure of 1kPa-10kPa to form a compact oxide film on the surface of the material, so as to obtain the composite material. The prepared composite material is good in thermal conductivity, thermal shock resistance and corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

technical field

[0001] The invention relates to the technical field of aluminum electrolysis waste heat recovery, in particular to a composite material used for recovery of aluminum electrolysis waste heat from flue gas and a preparation method thereof. Background technique

[0002] Electrolytic aluminum is a high-energy-consuming industry. In the production process of primary aluminum, each ton of aluminum consumes about 13,000kW·h of electricity, but only about 50% of the electricity is used to maintain the normal progress of the electrolysis process, and the remaining about 50% of the electricity is used as heat. loss of form. Therefore, if the waste heat generated in the aluminum electrolysis process is not reused, not only the energy utilization rate is reduced, but also the production environment is deteriorated. Therefore, it is necessary to recover the waste heat generated in the aluminum electrolysis process and improve the energy use efficiency.

[0003] Studies h...

Examples

Embodiment 1

[0040] NiO and Fe 2 o 3 According to the molar ratio of 0.5:1, mix evenly into the ball mill, use ethanol as the ball milling medium for 1h, and then mix NiO and Fe 2 o 3 After the mixture is dried, put it into a resistance furnace, and use N 2 as a protective atmosphere while maintaining O 2 The partial pressure is 15kPa, and it is calcined at 1050°C for 4h to obtain spinel Ni 0.6 Fe 2.4 o 4 powder. Among them, the NiO and Fe used 2 o 3 The particle size is 50-200 mesh, and the purity is above 99%.

[0041] The resulting spinel Ni 0.6 Fe 2.4 o 4 Powder and metal fiber or alloy fiber, non-spinel oxide, carbide, nitride, boride are added to the ball mill and mixed evenly, wherein, the specific composition of each component and the mass fraction of the raw material are:

[0042] Spinel oxide: Ni 0.6 Fe 2.4 o 4 38%;

[0043] Metal fiber or alloy fiber: Cu 25%, Co 13%;

[0044] Non-spinel oxides: CaO 3%, TiO 2 2%, BaO 2% and CeO 2 2%;

[0045] Carbide: TaC ...

Embodiment 2

[0052] Combine CoO and Fe 2 o 3 According to the molar ratio of 0.73:1, mix them evenly and add them to the ball mill, use ethylene glycol as the ball milling medium for 3 hours, and then put CoO and Fe 2 o 3 After the mixture was dried, it was placed in a resistance furnace with Ar as the protective atmosphere while maintaining O 2 The partial pressure is 20kPa, and it is calcined at 1150°C for 5h to obtain spinel Co 0.8 Fe 2.2 o 4 powder. Among them, the used CoO and Fe 2 o 3 The particle size is 50-200 mesh, and the purity is above 99%.

[0053] The resulting spinel Co 0.8 Fe 2.2 o 4 Powder and metal fiber or alloy fiber, non-spinel oxide, carbide, nitride, boride are added to the ball mill and mixed evenly, wherein, the specific composition of each component and the mass fraction of the raw material are:

[0054] Spinel oxide: Co 0.8 Fe 2.2 o 4 38%;

[0055] Metal fiber or alloy fiber: Ni 24%, Fe 12%;

[0056] Non-spinel oxides: MgO 4.5%, SnO 2 3.5%, Ag...

Embodiment 3

[0064] NiO and Al 2 o 3 According to the molar ratio of 1:1, mix evenly into the ball mill, use water as the ball milling medium for 2 hours, and then mix NiO and Al 2 o 3 After the mixture is dried, put it into a resistance furnace, and use N 2 as a protective atmosphere while maintaining O 2 The partial pressure is 25kPa, and it is calcined at 1250°C for 6h to obtain spinel NiAl 2 o 4 powder. Among them, the NiO and Al used 2 o 3 The particle size is 50-200 mesh, and the purity is above 99%.

[0065] The obtained spinel NiAl 2 o 4 Powder, metal fibers or alloy fibers, non-spinel oxides, carbides, nitrides, and borides are added to the ball mill and mixed evenly. Among them, the specific composition of each component and the mass fraction of the raw materials are:

[0066] Spinel oxide: NiAl 2 o 4 38%;

[0067] Metal fiber or alloy fiber: Ti 20%, Nb 16%;

[0068] Non-spinel oxide: V 2 o 5 4%, NiO 2.5%, PbO 2 3.5% and La 2 o 3 2%;

[0069] Carbide: AlC...